Chromium-containing collagen waste dechroming method based on collagen expansion inhibition and application of chromium-containing collagen waste dechroming method
Through the combined use of alkali treatment and non-swelling acid solubilizer, the expansion of collagen is inhibited, dehydration is improved, the problem of difficult separation of chromium and collagen and high degree of hydrolysis is solved, and efficient dechromization effect and recovery of chromium resources are achieved.
Patent Information
- Application Number
- CN202410954848.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-16
AI Technical Summary
In the existing dechromization technology for chromium-containing collagen waste, it is difficult to separate chromium and collagen, the dechromization rate is not high, and the hydrolysis of collagen is too high, resulting in unsatisfactory dechromization effects and difficulty in recycling chromium.
Chromium hydroxide precipitate is formed through alkali treatment, and non-swelling acid solubilizers such as phenolsulfonic acid are added to inhibit collagen expansion, improve dehydration, achieve efficient separation of chromium and collagen, and reduce the degree of collagen hydrolysis.
It significantly increases the dechromization rate, obtains dechromized collagen fibers with a complete structure, reduces the chromium content in the waste liquid, simplifies the treatment process, and achieves efficient recovery of chromium resources and high-value utilization of collagen fibers.
Abstract
Description
Technical Field
[0001] The invention relates to a leather waste treatment technology, in particular to an efficient chromium removal method for chromium-containing collagen waste based on collagen expansion inhibition, and belongs to the field of solid waste treatment. Background Art
[0002] During the mechanical processing of trimming, shaving, grinding and other processes after chrome tanning, a large amount of chromium-containing collagen waste will be generated. Chromium-containing collagen waste contains about 90% collagen and 2.0%-4.0% Cr(III). Fully removing Cr(III) from chromium-containing solid waste and achieving efficient separation and recovery of collagen and chromium is an effective way to achieve high-value utilization of chromium-containing collagen waste.
[0003] At present, the reported methods for removing chromium from chromium-containing collagen waste can be divided into high hydrolysis method and low hydrolysis method according to the degree of collagen hydrolysis. The high hydrolysis method treats chromium-containing collagen waste with acid, alkali and / or enzyme at a relatively high temperature to highly hydrolyze the collagen fibers, release Cr(III) and further convert it into Cr(OH)3 precipitate, and separate the soluble collagen hydrolysate and the chromium precipitate through operations such as filter pressing. However, the molecular weight of the collagen hydrolysate obtained by this method is low, and its application value is greatly reduced. For example, the alkaline method used in Chinese Patent ZL 202010188510.1 for removing chromium can only obtain small-molecule collagen hydrolysate.
[0004] The main methods for dechroming with low hydrolysis degree are oxidation method and ligand replacement method. The oxidation method oxidizes Cr(III) into Cr(VI) which has no binding properties with collagen, so as to separate chromium from collagen fibers. For example, in Chinese patent ZL 02113818.4, multiple oxidation dechroming is performed under the action of ultrasound, and the dechroming rate can reach 99%. However, due to the difficulty in treating the wastewater containing Cr(VI), this method is difficult to promote and apply. The ligand replacement method refers to replacing the collagen carboxyl group bound to Cr(III) with a ligand with strong coordination ability with Cr(III) to generate a new water-soluble chromium complex, so that the chromium ions are removed from the collagen fibers, thereby achieving the purpose of dechroming. The collagen fibers after dechroming by this method can maintain a relatively complete original structure. Chinese patent ZL 201910762374.X introduces a step-by-step combined dechromization method using organic acids and organic acid salts, with a dechromization rate of up to 99.6%. However, the large amount of organic acids and salts used enhances the stability of the Cr(III) complex in the wastewater, making it more difficult to treat chromium-containing wastewater to meet standards, and making it difficult to achieve efficient recycling of Cr(III). - The coordination ability with Cr(III) is the strongest, so OH -It can replace the collagen coordinated with Cr(III) to the greatest extent to form chromium hydroxide precipitation, and then use acid to dissolve the precipitation, so as to achieve the separation of chromium and collagen fibers. However, during the acid dissolution and precipitation process, collagen easily absorbs water and swells, making it difficult to achieve efficient separation of chromium-containing waste liquid and collagen fibers, and failing to achieve the ideal chromium removal effect. In addition, collagen in a swollen state is more easily hydrolyzed, resulting in a high organic matter content in the waste liquid, which will further be detrimental to the recovery and utilization of chromium in the waste liquid. Summary of the invention
[0005] The purpose of the present invention is to provide a high-efficiency chromium removal method for chromium-containing collagen waste based on improving the chromium removal effect by inhibiting collagen expansion during acid-base treatment to improve the dehydration of collagen fibers, in view of the problems existing in the existing chromium removal technology for chromium-containing collagen waste, such as the difficulty in separating chromium and collagen, the chromium removal rate not meeting the requirements, and the high degree of hydrolysis of collagen.
[0006] The basic characteristics of the present invention are that chromium-containing collagen is first treated with alkali to form chromium hydroxide precipitation from chromium ions combined with skin collagen, and then non-swelling acid such as phenolsulfonic acid is added to dissolve the chromium hydroxide, and the swelling of collagen fibers can be inhibited, the dehydration of collagen fibers can be improved, and the separation of chromium-containing waste liquid and collagen fibers in the subsequent filter pressing process can be facilitated, and the chromium removal rate can be significantly improved. At the same time, the swelling inhibition effect can effectively reduce the hydrolysis degree of collagen during the acid treatment process.
[0007] The present invention provides a method for removing chromium from chromium-containing collagen waste based on collagen expansion inhibition to achieve the above-mentioned purpose, comprising the following steps, wherein the materials used in each step are calculated by weight:
[0008] 100 parts of chromium-containing collagen waste are put into a reactor, 500-3000 parts of water and 0-10 parts of rewetting agent are added, stirred at 20-40°C for 1-24 hours, 0-20 parts of neutral salt are added, stirred for 1-10 hours; 10-100 parts of alkaline solution are added to make the pH value of the bath liquid at 11.5-13.5, stirred for 1-24 hours; 10-100 parts of non-swelling acid solution are added to make the pH value of the bath liquid at 1.0-2.0, stirred for 1-24 hours; after filter pressing, 50-3000 parts of water, 0-20 parts of neutral salt, 0-10 parts of non-swelling acid are added, stirred for 1-6 hours, and filter pressed again to obtain dechromed collagen fibers.
[0009] In the above technical solution, the above operation can be repeated 1-3 times.
[0010] In the above technical scheme, the neutral salt is at least one of sodium chloride, sodium sulfate and potassium sulfate, the base is at least one of sodium hydroxide, calcium hydroxide, potassium hydroxide and lithium hydroxide, and the acid is at least one of phenolsulfonic acid, naphthalenesulfonic acid, naphthalene disulfonic acid, sulfonesulfonic acid and sulfosalicylic acid.
[0011] The above technical solution describes a method for dechroming chromium-containing collagen waste based on collagen expansion inhibition. The chromium-containing collagen waste is chromium-containing shavings or chromium-containing leather blocks produced during the leather making process. The dechromed collagen fibers can be used as raw materials for preparing collagen-based industrial products such as industrial gelatin.
[0012] Compared with the prior art, the present invention has the following advantages:
[0013] The present invention provides a method for dechroming chromium-containing collagen waste based on collagen swelling inhibition, which utilizes the swelling inhibition effect of non-swelling acid on collagen fibers to improve the dehydration of dechromed collagen fibers, realizes efficient separation of chromium-containing waste liquid and collagen fibers during filter pressing, significantly improves the dechroming rate, and the chromium content of the dechromed collagen fibers can reach below 50 mg / kg.
[0014] The present invention provides a method for dechroming chromium-containing collagen waste based on collagen expansion inhibition. The acid expansion inhibition of collagen fibers can significantly reduce the hydrolysis degree of collagen fibers, obtain dechromed collagen fibers with relatively complete structures, and expand the application range of the dechromed collagen fibers.
[0015] The invention provides a method for dechroming chromium-containing collagen waste based on collagen expansion inhibition. The materials used in the dechroming process are non-oxidizing, no toxic hexavalent chromium is generated, and no new pollution is generated.
[0016] The present invention provides a method for dechroming chromium-containing collagen waste based on collagen expansion inhibition. The materials used in the dechroming process hardly affect the precipitation performance of chromium in the dechroming waste liquid. The waste liquid can meet the emission standards after simple treatment, and the chromium resources recovered after precipitation can be well reused in leather tanning, etc.
[0017] 5. The present invention provides a method for removing chromium from chromium-containing collagen waste based on collagen expansion inhibition. The required equipment and operation steps are simple, and the tanneries can use existing conventional equipment for treatment, which has low cost and strong operability. DETAILED DESCRIPTION
[0019] The present invention is described in detail below through examples. It is necessary to point out that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments based on the above content of the present invention. The source of the materials used, the trade name and the components thereof are indicated when they first appear.
[0020] Example 1: Dander
[0021] 10 kg of chromium-containing shaved leather (cowhide), the dechroming method steps are as follows:
[0022] (1) Wash the chromium-containing shavings in the reactor once, drain the liquid, add 50 kg of water, and rotate for 24 hours.
[0023] (2) Add 1 kg of sodium sulfate to the bath solution in step (1), rotate for 1 h to fully dissolve it, then add 2 kg of sodium hydroxide solution (20%, w / w), and stir at room temperature for 6 h.
[0024] (3) Add 2.5 kg of naphthalene disulfonic acid solid to the bath solution in step (2), stir at room temperature for 6 h, and filter press.
[0025] (4) Add 2 kg of sodium sulfate, 0.5 kg of naphthalene disulfonic acid and 100 kg of water into a reactor, then add the chromium-containing shavings treated in step (3), stir at room temperature for 2 h, and filter.
[0026] (5) Repeat the above operation once for the chromium-containing shavings treated in step (4).
[0027] Example 2: Leather Block
[0028] 10 kg of chromium-containing leather (cowhide), the dechroming method steps are as follows:
[0029] (1) Add 150 kg of water to the reactor containing chromium leather and rotate for 24 h.
[0030] (2) Add 3 kg of sodium hydroxide solution (20%, w / w) to the bath solution in step (1) and stir at room temperature for 6 h.
[0031] (3) Add 6 kg of sulfone sulfonic acid solution (50%, w / w) to the bath solution in step (2), stir at room temperature for 12 h, and filter press.
[0032] (4) Add 1 kg of sulfone sulfonic acid solution (50%, w / w) and 150 kg of water into the reactor, then add the chromium-containing leather block treated in step (3), stir at room temperature for 2 h, and filter.
[0033] (5) Repeat the above operation once for the chromium-containing leather block treated in step (4).
Claims
1. A method for removing chromium from chromium-containing collagen waste based on collagen expansion inhibition, characterized in that The method comprises the following steps, and the materials used in each step are calculated by weight: 100 parts of chromium-containing collagen waste are put into a reactor, 500-3000 parts of water and 0-10 parts of rewetting agent are added, stirred at 20-40°C for 1-24 hours, 0-20 parts of neutral salt are added, stirred for 1-10 hours; 10-100 parts of alkaline solution are added to make the pH value of the bath liquid at 11.5-13.5, stirred for 1-24 hours; 10-100 parts of non-swelling acid solution are added to make the pH value of the bath liquid at 1.0-2.0, stirred for 1-24 hours; after filter pressing, 50-3000 parts of water, 0-20 parts of neutral salt, 0-10 parts of non-swelling acid are added, stirred for 1-6 hours, and filter pressing again to obtain dechromium collagen fibers; The above operation can be repeated 1-3 times.
2. The method for removing chromium from chromium-containing collagen waste based on collagen swelling inhibition according to claim 1, characterized in that The neutral salt is at least one of sodium chloride, sodium sulfate and potassium sulfate.
3. The method for removing chromium from chromium-containing collagen waste based on collagen swelling inhibition according to claim 1, characterized in that The alkali is at least one of sodium hydroxide, calcium hydroxide, potassium hydroxide and lithium hydroxide.
4. The method for removing chromium from chromium-containing collagen waste based on collagen swelling inhibition according to claim 1, characterized in that The acid is at least one of phenolsulfonic acid, naphthalenesulfonic acid, naphthalene disulfonic acid, sulfonesulfonic acid and sulfosalicylic acid.
5. A method for dechroming chromium-containing collagen waste based on collagen expansion inhibition and its application according to claims 1-4, characterized in that The chromium-containing collagen waste is chromium-containing shavings or chromium-containing leather blocks produced during the leather making process, and the dechromed collagen fibers can be used as raw materials for preparing collagen-based industrial products such as industrial gelatin.
Citation Information
Patent Citations
Method for recovering collagen and chromium salts from chromium-containing scrap leather residues
CN103014191A
Method for detoxifying chromium slag and recycling compound by hydrothermal reduction through abandoned biomass
CN107739831A
Preparation method of non-acid-soaking chrome tanning agent
CN109852741A
No-pickling chrome tanning agent
CN109880942A
Novel process for resource regeneration and utilization of wet blue leather of leather leftovers after dechroming
CN110438271A