Cold pressing method for reducing residual stress of ultra-large aluminum alloy integral frame die forging

By designing a specific cold pressing die structure and process during the cold pressing process of ultra-large aluminum alloy integral frame die forgings, the problems of excessive load, poor stress transfer effect and poor die matching are solved, and the method of effectively reducing residual stress is achieved. The effect ensures the control of part deformation.

CN118751833AActive Publication Date: 2024-10-11CHINA NAT ERZHONG GRP DEYANG WANHANG DIE FORGING CO LTD

Patent Information

Application Number
CN202411040767.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-11
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Super large aluminum alloy integral frame die forgings have problems such as excessive load, poor stress transfer effect and poor mold matching during the cold pressing process, making it difficult to effectively reduce residual stress and control part deformation.

Method used

A new cold pressing method is designed. By modeling the forging model in a three-dimensional modeling software, and designing the cold pressing die based on the model, the top of the cold-pressed high-rib cavity is a positive gap relative to the top of the high-rib forging. The cold-pressed web cavity has a positive gap relative to the forging web plate, and the top of the cold-pressed low rib cavity has a negative gap relative to the low rib top of the forging. Combined with special simulation software to calculate the residual stress and cold pressing load, the cold pressing mold is optimized to achieve Effective cold pressing process.

Benefits of technology

It effectively reduces the residual stress of super large aluminum alloy integral frame die forgings, reduces the cold pressing deformation force, improves the matching between cold pressing dies and forgings, and ensures the control of part deformation, especially on high and narrow outer edges. The high ribs allow the material to flow to the top of the ribs, eliminating residual stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751833A_ABST
    Figure CN118751833A_ABST
Patent Text Reader

Abstract

The invention discloses a cold pressing method for reducing residual stress of an ultra-large aluminum alloy integral frame die forging, belongs to the field of die forging residual stress control, and aims to effectively reduce the residual stress. The inner side face and the outer side face of a forge piece high rib of the forge piece model are planes with pattern draft. The cavity top of the high rib cavity of the cold pressing die designed according to the forge piece model is a positive gap relative to the rib top of the forge piece high rib; the side surface of the cold-pressed high rib cavity is a negative gap relative to the side surface of the forge piece high rib; the cold pressing web cavity is a positive gap relative to the forge piece web; and the cavity top of the cold-pressure low rib cavity is a negative gap relative to the rib top of the forge piece low rib. Optimizing a cold pressing die; forge piece forging is carried out through the cold pressing die. The projection area of the pressure-bearing surface in the movement direction of the press is smaller than that of a direct rib pressing top, so that the cold pressing deformation force is smaller. A negative gap is formed between the cold pressing die and the high-rib side wall of the forge piece model, the position of the forge piece is directly locked during cold pressing, and the cold pressing positioning matching problem does not need to be considered. The side wall is subjected to cold pressing, so that the material flows to the rib top, and the residual stress of the core of the outer edge strip is effectively eliminated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of residual stress control of die forgings, and specifically relates to a cold pressing method for reducing the residual stress of super-large aluminum alloy integral frame die forgings. Background Art

[0002] Super-large aluminum alloy integral frame die forgings refer to die forgings with a projected area greater than 5㎡. At present, due to the limited technology for controlling residual stress, domestic OEMs generally use pre-stretched plates to process super-large aluminum alloy integral frame parts, and super-large aluminum alloy integral frame die forgings have not been effectively applied. After the residual stress of the pre-stretched plate is reduced by stretching, the residual stress is controllable and the risk of deformation of the processed parts is low. However, at the same time, the pre-stretched plate has problems such as low performance abundance, fiber streamline truncation, and low material utilization. Therefore, the development of super-large aluminum alloy integral frame die forgings is extremely necessary. For medium and small aluminum alloy die forgings, the TXX52 (traditional cold pressing method) process is usually used to reduce residual stress (see Figure 1 , the blue line is the cold pressing die 2, and the black line is the forging model). However, for the ultra-large aluminum alloy integral frame die forgings with crisscross rib structures, this method has the following problems:

[0003] 1. Excessive load: When the traditional method is applied to cold pressing of ultra-large aluminum alloy integral frame die forgings, the contact area between the die (or tooling) and the forging is too large, the cold pressing load is too large, and generally the specified cold pressing deformation cannot be achieved;

[0004] 2. Poor stress transfer effect: The ribs of the integral frame beam forgings are thin and high, and the stress transfer efficiency is low when the ribs are cold pressed, which cannot achieve the purpose of reducing the residual stress in the core of the forging ribs (parts area);

[0005] 3. Poor die matching: When traditional cold pressing schemes (including but not limited to TXX52) are applied to simple forgings, it is easy to match the forgings with the cold pressing dies (tooling). However, for ultra-large aluminum alloy integral frame die forgings, the criss-crossing ribs, web structure, and thermal scaling coefficient fluctuations under actual working conditions all bring great difficulties to the matching of forgings with the cold pressing dies (tooling).

[0006] In view of this, the applicant intends to propose a new cold pressing scheme, which uses the residual stress trend as the principle indicator to overcome the shortcomings of the cold pressing process and effectively achieve the purpose of controlling the deformation of parts. Summary of the invention

[0007] The purpose of the present invention is to provide a cold pressing method for reducing the residual stress of ultra-large aluminum alloy integral frame die forgings, effectively reducing the residual stress, reducing the cold pressing deformation tonnage, and achieving the purpose of controlling the deformation of parts.

[0008] The technical solution adopted by the present invention is: a cold pressing method for reducing the residual stress of an ultra-large aluminum alloy integral frame die forging, comprising the following steps:

[0009] Step 1: Model a forging model in a 3D modeling software according to the overall frame part design, wherein the forging model includes a forging high rib, a forging belly plate and a forging low rib; the forging model performs complete feature design on the forging high rib, and both the inner side and the outer side of the forging high rib are planes with a draft angle; the inner side of the forging high rib and the forging belly plate are in a circular arc transition, and the outer side of the forging high rib and the forging belly plate are in a circular arc transition;

[0010] Step 2, designing a cold pressing die according to the forging model, the cold pressing die comprising a cold pressing high rib cavity corresponding to the forging high rib of the forging model, a cold pressing web cavity corresponding to the forging web, and a cold pressing low rib cavity corresponding to the forging low rib; the cavity top of the cold pressing high rib cavity has a positive gap relative to the rib top of the forging high rib; the inner side surface of the cold pressing high rib cavity has a negative gap relative to the inner side surface of the forging high rib; the outer side surface of the cold pressing high rib cavity has a negative gap relative to the outer side surface of the forging high rib; the cold pressing web cavity has a positive gap relative to the forging web; the cavity top of the cold pressing low rib cavity has a negative gap relative to the rib top of the forging low rib;

[0011] Step 3: After the forging model and cold pressing die are designed, special simulation software is used to calculate the residual stress state and cold pressing load of the forging after quenching and cold pressing unloading using the cold pressing die. Based on this, the cold pressing die is optimized in small quantities according to the equipment limit capacity;

[0012] Step 4: Implement forging, solution quenching and cold pressing processes according to the final forging model and cold pressing die, and inspect the deformation of the parts after processing them according to the solidification processing technology.

[0013] Furthermore, the forging web includes a forging close-distance web adjacent to the forging high ribs and a forging long-distance web away from the forging high ribs; the cold-pressed web cavity includes a cold-pressed close-distance web cavity adjacent to the cold-pressed high rib cavity and a cold-pressed long-distance web cavity away from the cold-pressed high rib cavity; the cold-pressed close-distance web cavity is equivalent to a positive gap of the forging close-distance web; the cold-pressed long-distance web cavity is flush with the cold-pressed low rib cavity.

[0014] Furthermore, the draft angle plane retention width of the forging model is ≥20 mm, and the draft angle is 5 to 10°.

[0015] Furthermore, the positive clearance between the cavity top of the cold pressing die and the top plane of the outer edge rib of the forging is ≥5mm; the negative clearance between the inner and outer plane areas of the outer edge rib of the cold pressing die and the forging model design is 2-3% of the outer edge rib thickness.

[0016] The beneficial effects of the present invention are as follows: First, according to the structural characteristics of the ultra-large integral frame die forgings, the present invention has a positive gap between the cavity top of the cold-pressed high-rib cavity and the rib top of the forging high rib, and the setting of the draft surface is smaller than that of the traditional TXX52 solution, and the projected area of ​​the pressure-bearing surface in the movement direction of the press is smaller than that of the direct pressing rib top, so the cold pressing deformation force is smaller. Especially for ultra-large integral frame die forgings, the forming force exceeding the limit capacity of the equipment is often a barrier to the effective reduction of residual stress.

[0017] Secondly, the cold pressing die of the traditional TXX52 cold pressing method is generally provided with a positive gap at the ribs and the ribs at the forging model. After the forging is placed on the cold pressing die, matching problems such as shaking and inaccurate positioning may occur. The present invention designs the cold pressing die and the high-rib side wall of the forging model to have a negative gap, that is, when the material is swung during the cold pressing process, the inclined surface of the forging near the top of the rib is in direct contact with the inclined surface of the cold pressing die near the bottom of the rib. At the same time, except for the high ribs, the remaining internal bottom ribs of the cold pressing die are not made into a rib web structure, so that the position of the forging can be directly locked during cold pressing, and there is no need to consider the cold pressing positioning matching problem.

[0018] Third, for high and narrow outer edge ribs, the traditional TXX52 cold pressing method cannot transfer plastic strain to the core of the edge bar, resulting in the inability to effectively eliminate the residual stress in the core of the edge bar. This solution can effectively eliminate the residual stress in the core of the outer edge bar by cold pressing the side wall to make the material flow to the top of the rib. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of the principle of traditional cold pressing;

[0020] Figure 2 This is a schematic diagram of the cross section of a typical forging of an ultra-large integral frame;

[0021] Figure 3 This is a schematic diagram of the cross section of a typical cold pressing die for an ultra-large integral frame;

[0022] Figure 4 It is a schematic diagram of position control during the cold pressing process;

[0023] Figure 5 This is a schematic diagram of the cold pressing principle of a typical forging of a super-large integral frame;

[0024] Figure 6 for Figure 5 A local enlarged view of point A;

[0025] Figure 7 for Figure 5 A partial enlarged view of point B.

[0026] In the figure, forging model 1, forging high rib 11, inner side 111, outer side 112, forging web 12, forging close-distance web 121, forging long-distance web 122, forging low rib 13, cold pressing die 2, cold pressed high rib cavity 21, cold pressed web cavity 22, cold pressed close-distance web cavity 221, cold pressed long-distance web cavity 222, cold pressed low rib cavity 23. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0028] A cold pressing method for reducing residual stress of an ultra-large aluminum alloy integral frame die forging comprises the following steps:

[0029] Step 1: Model the forging model 1 in the 3D modeling software according to the overall frame part design, such as Figure 2 As shown, the forging model 1 includes a forging high rib 11, a forging web 12 and a forging low rib 13; the forging model 1 performs complete feature design on the forging high rib 11, and the inner side surface and the outer side surface of the forging high rib 11 are both planes with a draft angle; the inner side surface of the forging high rib 11 and the forging web are in a circular arc transition, and the outer side surface of the forging high rib 11 and the forging web are in a circular arc transition.

[0030] Step 2: Design the cold pressing die 2 according to the forging model 1, such as Figure 3 As shown, the cold pressing die 2 includes a cold pressing high rib cavity 21 corresponding to the forging high rib 11 of the forging model 1, a cold pressing web cavity 22 corresponding to the forging web 12, and a cold pressing low rib cavity 23 corresponding to the forging low rib 13.

[0031] like Figure 5 , Figure 6 and Figure 7 As shown, the top of the cold-pressed high-rib cavity 21 has a positive gap relative to the top of the high rib 11 of the forged part, that is, the traditional TXX52 cold pressing scheme is not implemented on the forging. The inner side surface of the cold-pressed high-rib cavity 21 has a negative gap relative to the inner side surface of the high rib 11 of the forged part; the outer side surface of the cold-pressed high-rib cavity 21 has a negative gap relative to the outer side surface of the high rib 11 of the forged part. That is, the side wall of the forging model is cold-pressed by the wedge-shaped cold-pressing die 2. The cold-pressed web cavity 22 has a positive gap relative to the web 12 of the forged part; the top of the cold-pressed low-rib cavity 23 has a negative gap relative to the top of the low rib 13 of the forged part.

[0032] Step 3: After the forging model 1 and the cold pressing die 2 are designed, special simulation software is used to calculate the residual stress state and cold pressing load of the forging after quenching and cold pressing unloading using the cold pressing die 2. Based on this, the cold pressing die 2 is optimized in small quantities according to the equipment's limit capacity.

[0033] Step 4: Implement forging, solution quenching and cold pressing processes according to the finalized forging model 1 and cold pressing die 2, and inspect the deformation of the parts after processing them according to the solidification processing technology.

[0034] The forged web 12 includes a forged close-distance web 121 adjacent to the forged high rib 11 and a forged long-distance web 122 away from the forged high rib 11; the cold-pressed web cavity 22 includes a cold-pressed close-distance web cavity 221 adjacent to the cold-pressed high rib cavity 21 and a cold-pressed long-distance web cavity 222 away from the cold-pressed high rib cavity 21; the cold-pressed close-distance web cavity 221 is equivalent to a positive gap of the forged close-distance web 121; the cold-pressed long-distance web cavity 222 is flush with the cold-pressed low rib cavity 23.

[0035] In step one, according to the structural characteristics of the ultra-large aluminum alloy integral frame parts, it is generally a web structure of high outer ribs + short internal ribs. The forging model designed according to the part model must retain sufficient draft bevels while considering the smooth transition of the web ribs to be used for the pressure-bearing surface required for subsequent cold pressing production. Therefore, if the outer edge ribs of the part cannot meet this requirement under the normal increase in margin, the height margin of the outer edge ribs of the forging can be appropriately increased to ensure the smooth implementation of the subsequent new cold pressing scheme. The width of the pressure-bearing surface is determined by the height of the outer edge ribs and the draft angle, that is, the width of the pressure-bearing surface is also the draft length. It is worth noting that when the cold pressing is completed, the draft angle plane of the forging retains a width of ≥20 mm, and the draft angle is 5 to 10°.

[0036] In step 2, by designing the negative clearance of the outer edge side wall and the positive clearance of the rib top, the material flows to the rib top during the cold pressing process. At the same time, during the actual implementation of the cold pressing process, the high-rib side wall of the outer edge of the forging and the high-rib side wall of the outer edge of the cold pressing die are in surface contact, and the relative position of the forging is "locked" (see Figure 4 ), considering the forming force and the actual relative position of the internal ribs and webs of the forging, the internal short ribs are directly pressed using a plane to avoid mutual interference between the cold pressing die cavity and the internal ribs and webs of the forging shape. Preferably, the positive clearance value between the cavity top of the cold pressing high rib cavity 21 of the cold pressing die 2 and the top plane of the outer edge ribs of the forging is ≥5mm; the negative clearance value of the inner and outer plane areas of the outer edge high ribs of the cold pressing die 2 relative to the forging model design is 2-3% of the outer edge high rib thickness.

[0037] Example:

[0038] Taking an aluminum alloy integral frame forging as an example, the outer contour of the aluminum alloy integral frame forging is 3850×2000×230mm. The characteristic positions (mainly the outer edge high rib features and the internal rib web structure) are cut out at typical positions of the forging to make an integral frame die forging test piece.

[0039] The forging production process in this embodiment mainly includes die forging, solution quenching, cold pressing, aging, subsequent residual stress detection and parts processing. The specific process is as follows:

[0040] Step 1: The design of the integral frame die forging is determined by the method in step 1 above, and the integral frame die forging test piece is prepared based on this design. The test piece forging specification is 1000×700×230mm.

[0041] Step 2: A cold pressing mold 2 is designed in combination with the above step 2.

[0042] Step 3: Determine and optimize the cold pressing die model based on numerical simulation software simulation and complete the die production.

[0043] Step 4: Complete the production of forgings before cold pressing according to the specified die forging process and solution quenching process.

[0044] Step 5: Complete the cold pressing process of the forging according to the specified cold pressing process and the cold pressing die.

[0045] Step 6: Complete the final production of forgings according to the specified aging process.

[0046] Step 7: Perform residual stress test.

[0047] Step 8: Complete part processing and analyze part deformation.

[0048] Comparative example: Taking an aluminum alloy integral frame forging that is the same as the embodiment as an example, the outer contour of the aluminum alloy integral frame forging is 3850×2000×230mm. The characteristic positions (mainly the outer edge high rib features and the internal rib web structure) are cut at typical positions of the forging, and the integral frame die forging test piece is made by traditional cold pressing method.

[0049] The deformation conditions of the integral frame die forging test pieces made in the embodiment and the integral frame die forging test pieces made in the comparative example are shown in the following table:

[0050] Maximum deformation of outer edge ribs Maximum web deformation Comparative example (traditional TXX52) 0.365 0.33 Embodiment (cold pressing method of the present invention) 0.198 0.259

Claims

1. A cold pressing method for reducing residual stress of ultra-large aluminum alloy integral frame die forgings, characterized in that: The following steps are involved: Step 1: Model a forging model (1) in a three-dimensional modeling software according to the overall frame part design, wherein the forging model (1) includes a forging high rib (11), a forging web (12) and a forging low rib (13); the forging model (1) performs complete feature design on the forging high rib (11), and the inner side surface (111) and the outer side surface (112) of the forging high rib (11) are both planes with a draft angle; the inner side surface of the forging high rib (11) and the forging web are in a circular arc transition, and the outer side surface of the forging high rib (11) and the forging web are in a circular arc transition; Step 2: designing a cold pressing die (2) according to the forging model (1), wherein the cold pressing die (2) comprises a cold pressing high rib cavity (21) corresponding to the forging high rib (11) of the forging model (1), a cold pressing web cavity (22) corresponding to the forging web (12), and a cold pressing low rib cavity (23) corresponding to the forging low rib (13); The cavity top of the cold-pressed high-rib cavity (21) forms a positive gap with respect to the rib top of the forged high-rib (11); The inner side surface of the cold-pressed high-rib cavity (21) has a negative gap relative to the inner side surface of the forged high-rib (11); the outer side surface of the cold-pressed high-rib cavity (21) has a negative gap relative to the outer side surface of the forged high-rib (11); The cold-pressed web cavity (22) has a positive gap relative to the forged web (12); the top of the cold-pressed low rib cavity (23) has a negative gap relative to the top of the forged low rib (13); Step 3: After the forging model (1) and the cold pressing die (2) are designed, the residual stress state and the cold pressing load of the forging after quenching and cold pressing unloading using the cold pressing die (2) are calculated using a dedicated simulation software, and the cold pressing die (2) is optimized in small amounts based on this and according to the equipment limit capacity; Step 4: Implement forging, solution quenching and cold pressing processes according to the finalized forging model (1) and cold pressing die (2), and inspect the deformation of the parts after processing them according to the solidification processing technology.

2. The cold pressing method for reducing residual stress of ultra-large aluminum alloy integral frame die forgings according to claim 1, characterized in that: The forged web (12) comprises a forged short-distance web (121) adjacent to the forged high rib (11) and a forged long-distance web (122) away from the forged high rib (11); The cold-pressed web cavity (22) comprises a cold-pressed short-distance web cavity (221) adjacent to the cold-pressed high-rib cavity (21) and a cold-pressed long-distance web cavity (222) far from the cold-pressed high-rib cavity (21); The cold pressed close-distance web cavity (221) is equivalent to the close-distance web (121) of the forged piece as a positive gap; The cold-pressed long-distance web cavity (222) is flush with the cold-pressed low-rib cavity (23) and is the same cavity.

3. The cold pressing method for reducing residual stress of ultra-large aluminum alloy integral frame die forgings according to claim 2, characterized in that: The draft angle plane retention width of the forging model (1) is ≥20 mm, and the draft angle is 5-10°.

4. The cold pressing method for reducing residual stress of ultra-large aluminum alloy integral frame die forgings according to any one of claims 1 to 3, characterized in that: The positive clearance value between the cavity top of the cold pressing high rib cavity (21) of the cold pressing die (2) and the rib top plane of the outer edge of the forging is ≥5mm.

5. The cold pressing method for reducing residual stress of ultra-large aluminum alloy integral frame die forgings according to claim 4, characterized in that: The negative clearance value of the inner and outer plane areas of the outer edge high ribs of the cold pressing die (2) relative to the forging model design is 2-3% of the thickness of the outer edge high ribs.

Citation Information

Patent Citations

  • Method for eliminating residual stress after solid dissolution by oversize rib web plate type aluminum alloy die forging

    CN108315674A

  • Method for reducing residual stress of alloy plate part

    CN110158000A

  • Method for lowering quenched residual stress of high-strength aluminum large-scale frame-type die forging

    CN110468360A

  • Semi-finishing method for aluminum alloy die forging

    CN117020581A

  • Die for cold compression, and method for removing residual stress of stamp forging

    JP2003211248A

Cited By

  • Cold pressing method for reducing residual stress of rib plate type forgings

    CN120924886A