Method for brazing titanium alloy by using aluminum foil interlayer
By using aluminum foil as the intermediate layer solder, a TiAl2+TiAl full intermetallic compound joint is formed, which solves the problems of high cost, complex operation, and poor quality of titanium alloy welding, achieves low-cost, high-efficiency welding, and improves the quality of the welded joint. Corrosion resistance.
Patent Information
- Application Number
- CN202410921379.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
AI Technical Summary
Existing titanium alloy welding methods have problems such as high welding cost, complex operation, poor welding quality, and poor corrosion resistance.
Aluminum foil is used as the intermediate layer solder, and the TiAl2+TiAl full intermetallic compound joint is formed between the aluminum foil and the titanium alloy through vacuum brazing technology. The low cost and easy operation of the aluminum foil are used to improve the welding quality and corrosion resistance.
It significantly reduces the welding cost, simplifies the operation process, improves the welding efficiency and the corrosion resistance of the welded joint, forms a dense welding structure with small deformation, and achieves reliable welding of titanium alloys.
Smart Images

Figure CN118752028A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding, and in particular to a method for brazing a titanium alloy using an aluminum foil intermediate layer. Background Art
[0002] Titanium alloy has the advantages of high specific strength, good corrosion resistance and low density. It can meet the demand for lightweight structural parts and is widely used in aerospace and other fields.
[0003] With the continuous development of aerospace industry at home and abroad, the demand for titanium alloy structural parts in the industry is increasing, and the requirements for the welding quality of titanium alloy structural parts are becoming increasingly stringent. At present, the main welding methods for titanium alloy structural parts are tungsten inert gas welding, electron beam welding, laser welding, plasma arc welding and brazing. Among them, tungsten inert gas welding has strict requirements on the welding environment, and the consumption of argon gas during welding is large, resulting in high welding costs; electron beam welding is not suitable for welding workpieces with complex shapes; laser welding has strict requirements on the gap between workpieces; plasma arc welding is not suitable for welding curved workpieces. Brazing can achieve multi-layer welding and avoid the pollution of heat-affected zone and gas during fusion welding. Therefore, the research on the brazing process of complex titanium alloy structural parts has broad prospects.
[0004] At present, the commonly used brazing filler metals in the brazing process of titanium alloy structural parts mainly include three categories: silver-based, aluminum-based and titanium-based. Among them, silver-based brazing filler metals are very sensitive to chloride ions, resulting in poor corrosion resistance of titanium alloy structural parts; the melting point of titanium-based brazing filler metals is generally high, and it needs to be used above 900°C. High temperature can easily cause phase transformation of the base material during the brazing process, affecting the welding quality. The brazing temperature of aluminum-based brazing filler metals is low, and it is not easy to cause phase transformation of the titanium alloy base material. The titanium-aluminum compound formed by brazing has high corrosion resistance. However, the production cost of the commonly used aluminum-based brazing filler metals is high, and the operation is complicated, resulting in high welding costs. Therefore, it is urgent to study a welding method for titanium alloys with lower cost, simpler operation, reliable welding quality and stronger corrosion resistance. Summary of the invention
[0005] In order to solve the above technical problems, the technical solution adopted in this application is to provide a method for brazing titanium alloy using an aluminum foil intermediate layer, so as to solve the technical problems of high welding cost, complicated operation, poor welding quality and poor corrosion resistance existing in the existing titanium alloy welding method.
[0006] The present application embodiment provides a method for brazing titanium alloy using an aluminum foil intermediate layer, comprising the following steps:
[0007] (1) grinding, cleaning, and drying the aluminum foil to obtain a treated aluminum foil;
[0008] (2) grinding, cleaning, and drying the surface of the titanium alloy to be welded to obtain a treated titanium alloy;
[0009] (3) assembling the treated titanium alloy and the treated aluminum foil into a "sandwich structure" in the manner of "titanium alloy-aluminum foil-titanium alloy" to obtain a connection piece to be welded;
[0010] (4) placing the connecting piece to be welded into a brazing device, applying pressure to the connecting piece to be welded, and then heating it to the welding temperature for heat preservation treatment. After the heat preservation treatment is completed, cooling it to room temperature to obtain a titanium alloy weldment.
[0011] Preferably, in step (1), the thickness of the aluminum foil is 5 to 30 μm.
[0012] Preferably, in step (1), the aluminum foil is polished with sandpaper until the oxide layer on the surface of the aluminum foil is polished off.
[0013] Preferably, in step (1), the polished aluminum foil is immersed in an ethanol solution for ultrasonic cleaning, and the cleaning time is 10 to 25 minutes.
[0014] Preferably, in step (2), the titanium alloy surface to be welded is manually polished using 200#, 400#, 800#, and 1200# sandpapers in sequence until the surface is smooth.
[0015] Preferably, in step (2), the polished titanium alloy is immersed in acetone and ethanol solutions in sequence for ultrasonic cleaning, and the cleaning time is 10 to 25 minutes.
[0016] Preferably, in step (4), a pressure of 1000 to 2000 kPa is applied to the connection to be welded.
[0017] Preferably, in step (4), the connecting piece to be welded is heated at a heating rate of 5 to 15°C / min, and then heated to 800 to 900°C and kept warm for 10 to 25 minutes.
[0018] Preferably, in step (4), the brazing equipment includes a vacuum brazing furnace.
[0019] Preferably, in step (4), the weld joint of the titanium alloy weldment is a TiAl2+TiAl full intermetallic compound joint.
[0020] The present invention provides a method for brazing titanium alloy using an aluminum foil intermediate layer. The aluminum foil is used as the intermediate layer brazing material and a vacuum brazing method is used to form a TiAl2+TiAl full metal compound joint between the aluminum foil and the titanium alloy, thereby realizing reliable welding of the titanium alloy.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention uses aluminum foil as an intermediate layer to braze titanium alloy, and forms a TiAl2+TiAl full metal compound joint through the reaction between titanium and aluminum, thereby improving the welding quality and the corrosion resistance of the welded joint;
[0023] (2) The present invention uses aluminum foil to replace the existing aluminum-based solder, which significantly reduces the cost, is easy to operate, and improves the welding efficiency;
[0024] (3) Since the surface of the aluminum foil is very easy to form an oxide film, the present invention soaks the aluminum foil in an ethanol solution for ultrasonic cleaning to prevent oxidation of the aluminum foil, thereby improving the wettability of the aluminum foil on the titanium alloy surface, solving the technical problem that the oxide film on the metal surface has an adverse effect on the brazing process, and improving the welding quality and welding efficiency;
[0025] The invention has simple process, low cost, compact structure of brazed joint, small deformation, strong corrosion resistance and reliable welding. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0027] Figure 1 This is a schematic diagram of the assembly of the sandwich structure of "titanium alloy-aluminum foil-titanium alloy" in Example 1 of the present application;
[0028] Figure 2 This is a microstructure diagram of the weld joint of the titanium alloy weldment in Example 1 of the present application;
[0029] Figure 3 This is a microstructure diagram of the weld joint of the titanium alloy weldment in Example 2 of the present application;
[0030] Figure 4 This is a microstructure diagram of the weld joint of the titanium alloy weldment in Example 3 of the present application;
[0031] Figure 5 This is a microstructure diagram of the weld joint of the titanium alloy weldment in Example 4 of the present application;
[0032] Figure 6 This is a microstructure diagram of the weld joint of the titanium alloy weldment in Example 5 of the present application. DETAILED DESCRIPTION
[0033] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application clearer, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. The raw materials and devices used in the present invention, unless otherwise specified, are conventional commercial products; the methods used, unless otherwise specified, are conventional methods.
[0034] Example 1
[0035] This embodiment provides a method for brazing titanium alloy using an aluminum foil intermediate layer, comprising the following steps:
[0036] (1) Selecting an aluminum foil with a thickness of 10 μm, and grinding the aluminum foil with sandpaper until the oxide layer on the surface of the aluminum foil is polished off; then immersing the polished aluminum foil in an ethanol solution for ultrasonic cleaning for 20 minutes; after cleaning, drying the aluminum foil to obtain a treated aluminum foil;
[0037] (2) using 200#, 400#, 800#, and 1200# sandpaper to manually polish the surface of the titanium alloy to be welded until the surface is smooth; then immersing the polished titanium alloy in acetone and ethanol solutions for ultrasonic cleaning, the cleaning time is 20 minutes each; after cleaning, the titanium alloy is dried to obtain the treated titanium alloy;
[0038] (3) Assemble the treated titanium alloy and the treated aluminum foil into a "sandwich structure" in the manner of "titanium alloy-aluminum foil-titanium alloy" to obtain a connection piece to be welded; wherein the assembly schematic diagram of the "sandwich structure" is as follows: Figure 1 As shown;
[0039] (4) Place the connection piece to be welded in a vacuum brazing furnace, apply a pressure of 1000 kPa to the connection piece to be welded, and evacuate the vacuum brazing furnace to 5×10 -3 Pa, and then heat the welded connection piece at a heating rate of 10°C / min, heating to 800°C and then keeping it warm for 20 minutes; after the insulation treatment, cool it to room temperature with the furnace to obtain a titanium alloy weldment.
[0040] The microstructure of the welded joint of the titanium alloy weldment was obtained by microscopic observation using a scanning electron microscope (SEM). Figure 2 shown and in Figure 2 Some points were selected for energy spectrum (EDS) analysis, and the ratios of each element were obtained as shown in Table 1.
[0041] Example 2
[0042] The difference between this implementation method and Example 1 is that in step (1), the thickness of the aluminum foil is 5 μm, and the other steps are the same, and a titanium alloy weldment is finally obtained.
[0043] The welded joint of titanium alloy weldment was tested and its microstructure diagram was obtained as follows Figure 3 The ratio of each element is shown in Table 1.
[0044] Example 3
[0045] The difference between this implementation method and Example 1 is that in step (1), the thickness of the aluminum foil is 30 μm, and the other steps are the same, and a titanium alloy weldment is finally obtained.
[0046] The welded joint of titanium alloy weldment was tested and its microstructure diagram was obtained as follows Figure 4 The ratio of each element is shown in Table 1.
[0047] See also Figure 2 , 3 4. The weld joints of Examples 1 to 3 have dense structures, without any unwelded areas or cracks. A compound layer is formed between the middle layer of the aluminum foil and the titanium alloys on both sides. The weld width is uniform, indicating that the aluminum foil and the titanium alloys on both sides form a good connection. As the thickness of the aluminum foil increases, the weld width also increases, but the weld structure does not show obvious changes. It can be seen that the increase in the thickness of the aluminum foil will cause the weld width to increase, but will not change the overall structure and composition of the weld.
[0048] Please refer to Table 1, which shows the EDS analysis results of each point in the microstructure diagram of Examples 1 to 3. Figure 2 , 3 , the ratio of each element at each point in 4.
[0049] Table 1 EDS analysis results of each point in the microstructure diagram of Examples 1 to 3 (atomic fraction)
[0050]
[0051] It can be seen from Table 1 that the welded joints formed by the brazing methods of Examples 1 to 3 are TiAl2+TiAl full intermetallic compound joints.
[0052] Example 4
[0053] The difference between this implementation method and Example 1 is that in step (4), the applied pressure is 1500 kPa, and the other steps are the same, and finally a titanium alloy weldment is obtained.
[0054] The welded joint of titanium alloy weldment was tested and its microstructure diagram was obtained as follows Figure 5 The ratio of each element is shown in Table 2.
[0055] Example 5
[0056] The difference between this implementation method and Example 1 is that in step (4), the applied pressure is 2000 kPa, and the other steps are the same, and finally a titanium alloy weldment is obtained.
[0057] The welded joint of titanium alloy weldment was tested and its microstructure diagram was obtained as follows Figure 6 The ratio of each element is shown in Table 2.
[0058] See also Figure 2 , 5 , 6. The weld joints of Examples 1, 4, and 5 have dense structures, without any unwelded areas or cracks. A compound layer is formed between the middle layer of the aluminum foil and the titanium alloys on both sides. The weld width is uniform, indicating that the aluminum foil and the titanium alloys on both sides form a good connection. As the applied pressure increases, the weld width is roughly the same, about 10 μm, and the weld structure does not show obvious changes. It can be seen that the applied pressure has little effect on the weld width and weld structure.
[0059] Please refer to Table 2, which shows the EDS analysis results of each point in the microstructure diagram of Examples 1, 4, and 5. Figure 2 , 5 , the ratio of each element at each point in 6.
[0060] Table 2 EDS analysis results of each point in the microstructure diagram of Examples 1, 4, and 5 (atomic fraction)
[0061]
[0062]
[0063] It can be seen from Table 2 that the welded joints formed by the brazing methods of Examples 1, 4, and 5 are TiAl2+TiAl full intermetallic compound joints.
[0064] In summary, the preferred brazing conditions for brazing titanium alloy using an aluminum foil intermediate layer are: the thickness of the aluminum foil is 5 to 30 μm, and the applied pressure is 1000 to 2000 kPa.
[0065] The present invention provides a method for brazing titanium alloy using an aluminum foil intermediate layer. The aluminum foil is used as the intermediate layer brazing material and a vacuum brazing method is used to form a TiAl2+TiAl full metal compound joint between the aluminum foil and the titanium alloy, thereby realizing reliable welding of the titanium alloy.
[0066] Compared with the prior art, (1) the present invention adopts aluminum foil as the intermediate layer to braze titanium alloy, and forms a TiAl2+TiAl full metal compound joint through the reaction between titanium and aluminum, thereby improving the welding quality and the corrosion resistance of the welded joint; (2) the present invention adopts aluminum foil to replace the existing aluminum-based brazing filler metal, which significantly reduces the cost, is easy to operate, and improves the welding efficiency; (3) since the surface of the aluminum foil is very easy to form an oxide film, the present invention soaks the aluminum foil in an ethanol solution for ultrasonic cleaning to prevent the oxidation of the aluminum foil, thereby improving the wettability of the aluminum foil on the surface of the titanium alloy, solving the technical problem that the oxide film on the metal surface has an adverse effect on the brazing process, and improving the welding quality and welding efficiency; the present invention has a simple process, low cost, dense brazed joint structure, small deformation, strong corrosion resistance, reliable welding, and can be widely used in the field of welding technology.
[0067] It should be noted that:
[0068] (1) In the above-mentioned embodiments 1 to 5, in step (1), the ultrasonic cleaning time of the aluminum foil is selected to be 20 minutes. This is only a preferred embodiment. In actual operation, the ultrasonic cleaning time of the aluminum foil can be 10 to 25 minutes, which can be selected according to actual conditions.
[0069] (2) In the above embodiments 1 to 5, in step (2), the ultrasonic cleaning time of the titanium alloy is selected to be 20 minutes. This is only a preferred embodiment. In actual operation, the ultrasonic cleaning time of the titanium alloy can be 10 to 25 minutes, which can be selected according to actual conditions.
[0070] (3) In the above embodiments 1 to 5, in step (4), the brazing equipment is a vacuum brazing furnace, which is only a preferred embodiment. In actual operation, the brazing equipment includes but is not limited to a vacuum brazing furnace. As long as the vacuum degree during brazing is 5×10 -3 It can be below Pa and can be selected according to actual conditions.
[0071] (4) In the above embodiments 1 to 5, in step (4), the heating rate of 10°C / min is selected to heat the connection to be welded. This is only a preferred embodiment. In actual operation, the heating rate of the connection to be welded can be 5 to 15°C / min, which can be selected according to actual conditions.
[0072] (5) In the above embodiments 1 to 5, in step (4), when heating the connecting piece to be welded, the heating temperature is selected to be 800°C and the insulation time is selected to be 20 minutes; this is only a preferred embodiment. In actual operation, the heating temperature can be 800 to 900°C and the insulation time can be 10 to 25 minutes, which can be selected according to actual conditions.
[0073] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A method for brazing titanium alloy using an aluminum foil intermediate layer, characterized in that: The following steps are involved: (1) grinding, cleaning, and drying the aluminum foil to obtain a treated aluminum foil; (2) grinding, cleaning, and drying the surface of the titanium alloy to be welded to obtain a treated titanium alloy; (3) assembling the treated titanium alloy and the treated aluminum foil into a "sandwich structure" in the manner of "titanium alloy-aluminum foil-titanium alloy" to obtain a connection piece to be welded; (4) placing the connecting piece to be welded into a brazing device, applying pressure to the connecting piece to be welded, and then heating it to the welding temperature for heat preservation treatment. After the heat preservation treatment is completed, cooling it to room temperature to obtain a titanium alloy weldment.
2. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 1, characterized in that: In step (1), the thickness of the aluminum foil is 5 to 30 μm.
3. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 1, characterized in that: In step (1), the aluminum foil is polished with sandpaper until the oxide layer on the surface of the aluminum foil is polished off.
4. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 3, characterized in that: In step (1), the polished aluminum foil is immersed in an ethanol solution for ultrasonic cleaning, and the cleaning time is 10 to 25 minutes.
5. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 1, characterized in that: In step (2), the titanium alloy surface to be welded is manually polished using 200#, 400#, 800#, and 1200# sandpapers in sequence until the surface is smooth.
6. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 5, characterized in that: In step (2), the polished titanium alloy is immersed in acetone and ethanol solutions in turn for ultrasonic cleaning, and the cleaning time is 10 to 25 minutes.
7. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 1, characterized in that: In step (4), a pressure of 1000 to 2000 kPa is applied to the connection piece to be welded.
8. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 1, characterized in that: In step (4), the connecting piece to be welded is heated at a heating rate of 5 to 15°C / min, and then kept warm for 10 to 25 minutes after being heated to 800 to 900°C.
9. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 8, characterized in that: In step (4), the brazing equipment includes a vacuum brazing furnace.
10. The method for brazing titanium alloy using an aluminum foil intermediate layer according to claim 1, characterized in that: In step (4), the weld joint of the titanium alloy weldment is a TiAl2+TiAl full intermetallic compound joint.
Citation Information
Cited By
Titanium alloy laser welding method based on ultrasonic vibration and microalloying cooperative regulation and control
CN121491537A