Reshaping and repairing process for wheel-mounted brake disc of motor train unit
Through the EMU wheel-mounted brake disc shaping and repair process, combined with hot shaping and cold shaping technology, the waste problem after the wheel disc is scrapped is solved, the wheel disc is effectively repaired and the life is extended, the operation and maintenance cost and waste are reduced, and the efficiency is improved. Repair efficiency and success rate.
Patent Information
- Application Number
- CN202410942324.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-11
AI Technical Summary
The life of EMU wheels is generally shorter than that of wheel-mounted brake discs, resulting in a waste of remaining life after the discs are scrapped. Moreover, the old discs and new wheels cannot be directly assembled, and there is a lack of effective repair technology, resulting in operation and maintenance pressure.
The EMU wheel-mounted brake disc shaping and repair process is adopted, including disassembly and cleaning, visual inspection, wear measurement, cold press shaping, hot press shaping, magnetic particle and ultrasonic flaw detection, unbalance measurement, code engraving, combined with hot shaping and cold shaping Shaping technology eliminates deformation and stress and improves the service life of the wheel.
Effectively repair old disks, extend service life, reduce waste, reduce operation and maintenance costs, improve repair efficiency and success rate, and significantly extend the service life of roulette disks.
Smart Images

Figure CN118752173A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wheel-mounted brake disc shaping and repairing, and in particular relates to a process for shaping and repairing wheel-mounted brake discs for electric train sets. Background Art
[0002] At present, the life of EMU wheels at home and abroad is generally shorter than that of wheel-mounted brake discs (hereinafter referred to as discs). When the wheel is worn to a limit or damaged, the disc is scrapped together with the wheel, but the remaining life of the scrapped disc is relatively long, resulting in great waste. Since the disc body is subjected to thermal and mechanical loads for a long time, there is a certain deformation of the disc body after disassembly, which will cause inconsistent stress state of fasteners during reassembly, and the disassembled old disc and new wheel cannot be directly assembled. However, there is currently no effective repair technology for old discs, which has caused a large amount of waste of discs and also caused huge pressure on vehicle operation and maintenance. Summary of the invention
[0003] The present invention aims to solve the problem that after the EMU wheels are worn to a limit, the wheel disc is scrapped along with the wheel, but the scrapped wheel disc has a long remaining life, thereby providing an EMU wheel-mounted brake disc shaping and repair process, completing the repair of the plastically deformed old disc, and achieving the reuse of the repaired old disc, reducing waste and saving the EMU operation and maintenance costs.
[0004] To achieve the above-mentioned purpose, the present invention provides a reshaping and repairing process for a wheel-mounted brake disc of an EMU, comprising the following steps:
[0005] Step 1: Before repairing, disassemble the wheel disc and wheel, and clean the mounting surface, heat dissipation ribs and bottom surface of the bolt holes of the disassembled wheel disc;
[0006] Step 2: Visually inspect the surface of the wheel disc and remove the wheel disc with cracks that penetrate the thickness of the friction ring;
[0007] Step 3: Measure the remaining wear and deformation of the wheel disc, and eliminate the wheel discs with excessive wear and the remaining wear less than one maintenance cycle;
[0008] Step 4: Use a press tool to tighten the deformed wheel disc through the tool bolts, make the disc body and the tool completely flat, then turn the friction surface of the wheel disc and completely eliminate concave surface wear, inclined surface wear and wave wear;
[0009] Step 5: Place the wheel disc on the cold shaping tooling, use a large-tonnage press to apply counter pressure displacement near the heat dissipation ribs of the inner ring of the wheel disc, and maintain the pressure for the set time;
[0010] Step 6: The cold-pressed wheel is flatly loaded into the heat treatment furnace in a stacked arrangement. A ring is used on the top of the wheel body to constrain the natural deformation of the wheel. The inner and outer diameters of the ring are equivalent to the wheel body. The weight is 1 ton. The wheel body and the ring are placed in the heat treatment furnace for hot pressing and shaping. Protective gas is added to the furnace during hot pressing and shaping. The hot shaping temperature is 525±20℃ and the hot shaping time is 5 hours. After hot shaping, the furnace is cooled and taken out of the furnace at a temperature below 300℃.
[0011] Step 7: Measure the deformation of the wheel disc after hot pressing and shaping. If the warping deformation of the wheel disc after hot pressing and shaping is between [-0.2mm and 0.2mm], the wave deformation is between [-0.2mm and 0.2mm], and the parallelism between the friction surface and the wheel mounting surface is ≤0.15, proceed to step 8. If there are any items that are not satisfied, proceed to step 5.
[0012] Step 8: Perform magnetic particle inspection and ultrasonic inspection on the wheel. If it meets the set requirements, proceed to step 9;
[0013] Step 9: Measure the imbalance of the wheel. If the imbalance value is not greater than 15 gm, it is determined to be a qualified wheel and proceed to step 10;
[0014] Step 10: The inspection unit code and production number are engraved on the outer circle of the qualified wheel;
[0015] Step 11: The qualified roulette wheel is assembled with the new wheel according to the assembly standards and processes of the new roulette wheel, and then the assembled roulette wheel is inspected.
[0016] Furthermore, step 1 also includes that the cleaning area must be free of dirt, dust and rust, the bottom surface of the bolt mounting hole and the wheel disc mounting surface must be clean and have a metallic luster, minor scratches are allowed, and local protrusions must be polished and removed.
[0017] Furthermore, the step 5 also includes that the back pressure displacement is controlled between 10mm and 25mm according to the different deformation amounts of the disc body, the holding time is controlled between 10s and 20s, and a certain amount of warping deformation must be reserved for the wheel disc after cold pressing and shaping, and the warping deformation is controlled between 0.1mm and 0.3mm.
[0018] The repair process of the EMU wheel disc combining hot shaping and cold shaping of the present invention mainly relies on traditional brake disc production and processing equipment. The repair process is simple to operate, the repair cost is controllable, it is suitable for batch repair of wheel discs, and can significantly improve the repair efficiency; the repair process combining hot shaping and cold shaping can effectively eliminate the residual stress of the disc body while repairing the deformation of the wheel disc, reduce the probability of crack initiation and expansion of the serving wheel disc, increase the service life of the wheel disc after repair, and thus make full use of the remaining service life of the wheel disc; compared with the direct cold shaping process, the repair process of the EMU wheel disc combining hot shaping and cold shaping is easier to control the deformation of the wheel disc and has a high success rate in repairing the wheel disc. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Process flow chart of wheel disc reshaping and repair. DETAILED DESCRIPTION
[0020] In order to better understand the purpose, structure and function of the present invention, the following is a further detailed description of a EMU wheel-mounted brake disc shaping and repairing process of the present invention in conjunction with the accompanying drawings.
[0021] Reference Figure 1 The shaping and repair process of the wheel mainly includes the following processes.
[0022] Step 1: Before repairing the roulette, disassemble the roulette and wheel; clean the installation surface, heat dissipation ribs and bottom of the bolt holes of the disassembled roulette. There must be no dirt, dust and rust on the cleaned parts. The bottom of the bolt installation hole and the roulette installation surface must be clean and have a metallic luster. Minor scratches are allowed, and local protrusions must be polished off.
[0023] Step 2: Visually inspect the disc surface and remove discs with cracks that penetrate the friction ring thickness.
[0024] Step 3: Measure the remaining wear and deformation of the wheel disc, and eliminate the wheel discs with excessive wear and those with remaining wear less than one maintenance cycle.
[0025] Step 4: Use a pressing tool to tighten the deformed wheel disc through the tool bolts, so that the disc body and the tool are completely flush, then turn the friction surface of the wheel disc and completely eliminate concave wear, inclined surface wear and wave wear.
[0026] Step 5: Place the wheel on the cold shaping tooling, and use a large-tonnage press to apply counter-pressure displacement near the heat dissipation ribs of the inner ring of the wheel. According to the different deformation amounts of the wheel body, the counter-pressure displacement is controlled between 10mm and 25mm, and the holding time is controlled between 10s and 20s. After cold pressing and shaping, a certain amount of warping deformation must be reserved for the wheel, and the warping deformation is controlled between [0.1mm and 0.3mm].
[0027] Step 6: After cold pressing and shaping, the wheel disc is flatly loaded into the heat treatment furnace in a stacked arrangement. A ring is used on the top of the disc to constrain the natural deformation of the wheel disc. The inner and outer diameters of the ring are equivalent to the disc body and the weight is 1 ton. The disc body and the ring are placed in the heat treatment furnace for hot pressing and shaping. During hot pressing and shaping, protective gas is added to the furnace. The hot shaping temperature is 525±20℃ and the hot shaping time is 5 hours. After hot shaping, the furnace is cooled and taken out of the furnace at below 300℃.
[0028] Step 7: Measure the deformation of the wheel disc after hot pressing. If the warping deformation of the wheel disc after hot pressing is between [-0.2mm and 0.2mm], the wave deformation is between [-0.2mm and 0.2mm], and the parallelism between the friction surface and the wheel mounting surface is ≤0.15, proceed to step 8. If there are any items that are not satisfied, proceed to step 5.
[0029] Step 8: The wheel that meets the shaping requirements is subjected to magnetic particle inspection and ultrasonic inspection. The magnetic particle inspection is carried out in accordance with the requirements of GB / T9444, and the ultrasonic inspection is carried out in accordance with the requirements of GB / T 7233.1. If it meets the standard requirements, proceed to step 9.
[0030] Step 9: Measure the imbalance of the repaired wheel. If the imbalance value is not greater than 15 gm, it is determined to be a qualified wheel and proceed to step 10.
[0031] Step 10: The maintenance unit code (or logo) and production number are engraved on the outer circle of the qualified wheel.
[0032] Step 11: The qualified roulette wheel is assembled with the new wheel according to the assembly standards and processes of the new roulette wheel, and then the assembled roulette wheel is inspected.
Claims
1. A process for shaping and repairing wheel-mounted brake discs of EMUs, characterized in that: The steps include: Step 1: Before repairing, disassemble the wheel disc and wheel, and clean the mounting surface, heat dissipation ribs and bottom surface of the bolt holes of the disassembled wheel disc; Step 2: Visually inspect the surface of the wheel disc and remove the wheel disc with cracks that penetrate the thickness of the friction ring; Step 3: Measure the remaining wear and deformation of the wheel disc, and eliminate the wheel discs with excessive wear and the remaining wear less than one maintenance cycle; Step 4: Use a press tool to tighten the deformed wheel disc through the tool bolts, make the disc body and the tool completely flat, then turn the friction surface of the wheel disc and completely eliminate concave surface wear, inclined surface wear and wave wear; Step 5: Place the wheel disc on the cold shaping tooling, use a large-tonnage press to apply counter pressure displacement near the heat dissipation ribs of the inner ring of the wheel disc, and maintain the pressure for the set time; Step 6: The cold-pressed wheel is flatly loaded into the heat treatment furnace in a stacked arrangement. A ring is used on the top of the wheel body to constrain the natural deformation of the wheel. The inner and outer diameters of the ring are equivalent to the wheel body. The weight is 1 ton. The wheel body and the ring are placed in the heat treatment furnace for hot pressing and shaping. Protective gas is added to the furnace during hot pressing and shaping. The hot shaping temperature is 525±20℃ and the hot shaping time is 5 hours. After hot shaping, the furnace is cooled and taken out of the furnace at a temperature below 300℃. Step 7: Measure the deformation of the wheel disc after hot pressing and shaping. If the warping deformation of the wheel disc after hot pressing and shaping is between [-0.2mm and 0.2mm], the wave deformation is between [-0.2mm and 0.2mm], and the parallelism between the friction surface and the wheel mounting surface is ≤0.15, proceed to step 8. If there are any items that are not satisfied, proceed to step 5. Step 8: Perform magnetic particle inspection and ultrasonic inspection on the wheel disc. If it meets the standard requirements, proceed to step 9; Step 9: Measure the imbalance of the wheel. If the imbalance value is not greater than 15 gm, it is determined to be a qualified wheel and proceed to step 10; Step 10: The inspection unit code and production number are engraved on the outer circle of the qualified wheel; Step 11: The qualified roulette wheel is assembled with the new wheel according to the assembly standards and processes of the new roulette wheel, and then the assembled roulette wheel is inspected.
2. The process for shaping and repairing a wheel-mounted brake disc of an EMU according to claim 1, characterized in that: The step 1 also includes that the cleaning area must be free of dirt, dust and rust, the bottom surface of the bolt mounting hole and the wheel disc mounting surface must be clean and have a metallic luster, minor scratches are allowed, and local protrusions must be polished and removed.
3. The process for shaping and repairing a wheel-mounted brake disc of an EMU according to claim 1 is characterized in that: The step 5 also includes that the back pressure displacement is controlled between 10mm and 25mm according to the different deformation amounts of the disc body, the holding time is controlled between 10s and 20s, and a certain amount of warping deformation must be reserved for the wheel disc after cold pressing and shaping, and the warping deformation is controlled between 0.1mm and 0.3mm.
Citation Information
Patent Citations
Flat circular basin frame production process
CN104028634A
Maintenance method for wheel-mounted brake disc
CN117340539A
Thermal correction repair method for wheel-mounted brake disc of high-speed motor train unit
CN117415242A
Method for repairing break of universal connecting rod of universal coupling
US20150368733A1