Super-large-wall-thickness longitudinal submerged arc welding steel pipe suitable for ocean low-temperature environment

By using low-alloy quenched and tempered steel plates and specific welding processes in low-temperature marine environments, the strength and toughness problems of ultra-large-wall-thickness longitudinal submerged arc welded steel pipes in the marine environment have been solved, and the mass production of high-strength and tough steel pipes has been achieved to meet the needs of High requirements of the marine environment and extended service life through anti-corrosion treatment.

CN118752177APending Publication Date: 2024-10-11HEFEI ZIKING PIPE INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410746313.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the low-temperature marine environment, it is difficult to produce ultra-large-walled straight-seam submerged arc welded steel pipes with high strength and good toughness using existing technology, and the welding process is complex and difficult to meet the high requirements of the marine environment for steel pipes.

Method used

By selecting a suitable low-alloy quenched and tempered steel plate, performing rolling and preheating treatment, using a single-wire submerged arc welding process with double-sided , achieve high strength and toughness, and extend service life through shot peening and anti-corrosion coating.

Benefits of technology

It has realized the mass production of ultra-large wall thickness straight seam submerged arc welded steel pipes, which have high strength, good plastic toughness and low temperature impact properties, meet the performance requirements of the marine environment, reduce production costs and improve economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004886553950000041
    Figure BDA0004886553950000041
  • Figure BDA0004886553950000042
    Figure BDA0004886553950000042
  • Figure BDA0004886553950000051
    Figure BDA0004886553950000051
Patent Text Reader

Abstract

The invention discloses an ultra-large-wall-thickness longitudinal submerged arc welding steel pipe suitable for an ocean low-temperature environment, relates to the technical field of steel pipe machining, and provides a preparation method of the ultra-large-wall-thickness longitudinal submerged arc welding steel pipe from the aspects of raw material steel plate selection and welding process formulation. And the steel pipe has relatively high strength, good plasticity and toughness and low-temperature impact performance, is stable and uniform in mechanical property, and can meet the requirements of marine environment on the use performance and high reliability of the steel pipe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel pipe processing, and in particular to an ultra-thick wall straight seam submerged arc welded steel pipe suitable for marine low-temperature environments. Background Art

[0002] As is known, the wall thickness of existing straight seam submerged arc welded steel pipes is mostly below 120mm, the production process is relatively mature, and problems are not prone to occur during the steel pipe rolling and welding process. Conventional hot-rolled or controlled-rolled steel plates are generally used without additional alloy elements. They have good weldability and are suitable for general environments.

[0003] In marine and low temperature environments, considering the load-bearing characteristics of steel pipes, steel pipes are required to have high bearing strength, and the method of using extra-large wall thickness will be used to increase the bearing capacity when designing important node structures. In addition, marine and low temperature environments require steel pipes to have certain corrosion resistance and good low-temperature toughness, and the performance of the entire welded joint is stable and uniform.

[0004] Since ultra-thick plates cannot be strengthened by conventional mechanical rolling, they can only be strengthened by adding alloy elements and heat treatment to achieve the required strength value, so low-alloy quenched and tempered steel is selected. Due to the strong tendency of thick-walled steel plates to harden and the softening of joints caused by quenched and tempered steel during welding, the production and welding of ultra-thick steel pipes are greatly increased. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a super thick wall (T max =150mm) straight seam submerged arc welded steel pipe has high strength and toughness, good bearing capacity, and meets the high requirements of marine environment and low temperature environment for the performance of steel pipe.

[0006] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:

[0007] The first object of the present invention is to provide a method for preparing an ultra-thickness longitudinal submerged arc welded steel pipe, comprising the following steps:

[0008] (1) Confirmation of chemical composition and properties of steel plates;

[0009] (2) Rolling the steel plate;

[0010] (3) Preheat the steel plate before welding, adopt submerged arc welding technology, the welding groove is a double-sided X-shaped groove, slow cooling and insulation after welding, and the interlayer temperature is controlled below 200℃.

[0011] The second object of the present invention is to provide an ultra-thickness straight seam submerged arc welded steel pipe prepared by the aforementioned preparation method.

[0012] The third object of the present invention is to provide the application of the aforementioned ultra-thickness longitudinal submerged arc welded steel pipe in a low-temperature marine environment.

[0013] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing an ultra-thickness straight seam submerged arc welded steel pipe from the aspects of raw material steel plate selection and welding process formulation, which can not only realize the mass production of ultra-thickness steel pipes, but also the steel pipe has high strength, good plasticity and toughness, and low-temperature impact performance, and stable and uniform mechanical properties, which can meet the requirements of the marine environment for the performance and high reliability of the steel pipe. DETAILED DESCRIPTION

[0014] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.

[0015] The present invention provides a method for preparing a super-thickness longitudinal submerged arc welded steel pipe, comprising the following steps:

[0016] (1) Confirmation of chemical composition and properties of steel plates;

[0017] (2) Rolling the steel plate;

[0018] (3) Preheat the steel plate before welding, adopt submerged arc welding technology, the welding groove is a double-sided X-shaped groove, slow cooling and insulation after welding, and the interlayer temperature is controlled below 200℃.

[0019] In a further technical solution, the steel plate includes the following components in mass percentage: Mn 1.32-1.60%, Si 0.15-0.48%, Ni 0.20-0.75%, Cr 0.06-0.25%, C 0.07-0.12%, Cu 0.03-0.19%, Mo0.01-0.05%, Alt 0.02-0.06%, Nb 0.016-0.03%, Ti0.007-0.02%, V 0.002-0.022%, P≤0.019%, N≤0.0062%, S≤0.006%, Ceq0.41-0.42%, Pcm 0.18-0.23%, and the balance is Fe and unavoidable impurities.

[0020] Quenched and tempered steel is made by adding alloy elements such as Cr, Ni, and Mo to ordinary carbon steel, so that the steel plate can obtain low-carbon martensite after quenching and obtain good comprehensive mechanical properties after tempering. Adding Cr and Mo to steel can improve the corrosion resistance of steel to a certain extent. Compared with ordinary low-carbon steel, quenched and tempered steel has high strength and good toughness. It can maintain good strength and toughness under large deformation, and has the advantages of good wear resistance, processing performance and corrosion resistance. The wall thickness of the steel plate is between 110-150mm to meet the load-bearing requirements of specific application environments.

[0021] In a further technical solution, the steel plate rolling method includes hot rolling method, cold rolling method, mechanical rolling method, etc. In the present invention, the steel plate is rolled using conventional processes.

[0022] In a further technical solution, the preheating temperature of the steel plate before welding ranges from 120 to 150°C.

[0023] In a further technical solution, the inner and outer depth ratio of the welding groove is 1:2, and the blunt edge is 2-3 mm. The present invention adopts a double-sided X-shaped welding groove, controls the groove depth ratio, balances the internal stress while reducing the amount of deposition, thereby reducing deformation and facilitating the subsequent rounding process.

[0024] In a further technical solution, the submerged arc welding is single-wire submerged arc welding. The heat input of the entire welding process is controlled at 2.18-2.68KJ / mm, and multi-layer and multi-pass welding is adopted to control the temperature between layers, and heat preservation and slow cooling after welding can effectively prevent cold crack defects after welding, reduce softening of the heat-affected zone, and ensure the performance of the entire welded joint.

[0025] In a further technical solution, the submerged arc welding uses low-Ni alloy welding wire and fluorine-alkali type flux. The low-Ni alloy welding wire and the matching fluorine-alkali type flux make the weld have good mechanical properties, ensuring uniform and stable performance of the entire welded joint, high strength and good toughness. The joint has been subjected to -40°C impact test and -10°C CTOD test, and the test results far exceed the requirements of industry specifications, and the post-weld stress relief heat treatment is eliminated, which improves production efficiency and reduces production costs, so that the mass production of thick-walled steel pipes can obtain good economic benefits.

[0026] The present invention provides an ultra-thickness straight seam submerged arc welded steel pipe prepared by the above-mentioned preparation method. max It can reach 150mm, which can meet the load-bearing requirements in special fields.

[0027] The present invention also provides the application of the aforementioned ultra-thickness longitudinal submerged arc welded steel pipe in a low-temperature marine environment. The low-temperature marine environment is a special application environment that requires the steel pipe to have not only good mechanical properties and processing properties, but also excellent low-temperature resistance.

[0028] Example 1

[0029] (1) Confirmation of chemical composition and properties of steel plates.

[0030] Table 1 Chemical composition of steel plate

[0031]

[0032]

[0033] On the basis of ordinary carbon steel, alloy elements such as Cr, Ni, and Mo are added to enable the steel plate to obtain low-carbon martensite after quenching and obtain good mechanical properties, processing properties, and corrosion resistance after tempering.

[0034] (2) The steel plate is rolled into a round shape by cold rolling, and the wall thickness of the steel plate is 150 mm.

[0035] (3) The steel plate was preheated before welding to a temperature of 122°C. The single-wire submerged arc welding process was adopted. The welding groove was a double-sided X-shaped groove with an inner and outer depth ratio of 1:2 and a blunt edge of 2-3 mm. The welding material was a combination of TUnion SA Ni1 submerged arc welding wire and UV C 418TT-M submerged arc welding flux from Aolian Steel Bole Welding (China) Co., Ltd. After welding, the steel plate was slowly cooled and kept warm, and the interlayer temperature was controlled below 200°C.

[0036] Product performance parameters are shown in Table 1:

[0037] Table 1

[0038]

[0039] Example 2

[0040] (1) Same as Example 1.

[0041] (2) The steel plate is rolled into a round shape by cold rolling, and the wall thickness of the steel plate is 150 mm.

[0042] (3) The steel plate is preheated before welding to a temperature of 123°C. The single-wire submerged arc welding process is adopted. The welding groove is a double-sided X-shaped groove with an inner and outer depth ratio of 1:2 and a blunt edge of 2-3 mm. The welding material is a combination of TSW-12KHG submerged arc welding wire and TF-210 submerged arc welding flux from Tiantai Welding Material Manufacturer. After welding, the steel plate is slowly cooled and kept warm, and the interlayer temperature is controlled below 200°C.

[0043] Product performance parameters are shown in Table 2:

[0044] Table 2

[0045]

[0046]

[0047] Example 3

[0048] (1) Same as Example 1.

[0049] (2) The steel plate is rolled into a round shape by a cold rolling method, and the wall thickness of the steel plate is 110 mm.

[0050] (3) The steel plate was preheated before welding to a temperature of 123°C. The single-wire submerged arc welding process was adopted. The welding groove was a double-sided X-shaped groove with an inner and outer depth ratio of 1:2 and a blunt edge of 2-3 mm. The welding material was TUnion SA Ni1 submerged arc welding wire + UV C 418TT-M submerged arc welding flux produced by Aolian Steel Bole Welding (China) Co., Ltd. After welding, the steel plate was slowly cooled and kept warm. The interlayer temperature was controlled below 200°C.

[0051] Product performance parameters are shown in Table 3:

[0052] Table 3

[0053]

[0054] The present invention also adds step (4) on the basis of the above technical solution, removing rust and pollutants on the surface of the steel pipe by shot peening, and effectively avoiding corrosion of the steel pipe by preparing an anti-corrosion coating to extend the service life of the steel pipe. That is, the present invention also provides another method for preparing an ultra-thickness straight seam submerged arc welded steel pipe, comprising the following steps:

[0055] (1) Confirmation of chemical composition and properties of steel plates;

[0056] (2) Rolling the steel plate;

[0057] (3) Preheat the steel plate before welding, adopt submerged arc welding technology, the welding groove is a double-sided X-shaped groove, slow cooling and insulation after welding, and the interlayer temperature is controlled below 200℃.

[0058] (4) The outer surface of the steel pipe is shot peened and anti-corrosion coating is prepared in sequence.

[0059] The preparation condition control parameters of steps (1)-(3) are the same as above.

[0060] In a further technical solution, the shot peening treatment is performed at a pressure of 0.5-0.8 MPa and for a time of 5-30 min.

[0061] In a further technical solution, the anti-corrosion coating is prepared from an anti-corrosion paint, which includes the following raw materials in parts by weight: 40-50 parts of phenolic epoxy resin, 25-35 parts of filler, 5-10 parts of active diluent, 1-5 parts of dispersant, 0.1-1 parts of defoaming agent, and 10-20 parts of curing agent.

[0062] Preferably, the active diluent is one or more of trimethylolpropane triglycidyl ether, 1,4-butanediol diglycidyl ether, and 1,6-hexanediol diglycidyl ether.

[0063] Preferably, the filler is selected from one or more of kaolin, wollastonite powder, titanium dioxide, talc powder and mica powder.

[0064] Preferably, the defoaming agent is a polyether defoaming agent.

[0065] Preferably, the curing agent is 1-(2-hydroxyethyl)-5-aminopyrazole. In the art, aliphatic amines, aromatic amines, alicyclic amines, and polyamides are usually used as epoxy resin curing agents to catalyze the curing reaction of epoxy resins, promote cross-linking reactions of epoxy resin molecules, generate a three-dimensional network structure, make epoxy resins solid, and adjust the application properties of epoxy resins. The present invention uses 1-(2-hydroxyethyl)-5-aminopyrazole as a curing agent, which can not only reduce the amount of curing agent used, but also effectively improve the application properties of epoxy resins.

[0066] Example 4

[0067] (1) Same as Example 1.

[0068] (2) The steel plate is rolled into a round shape by cold rolling, and the wall thickness of the steel plate is 150 mm.

[0069] (3) The steel plate is preheated before welding to a temperature of 123°C. The single-wire submerged arc welding process is adopted. The welding groove is a double-sided X-shaped groove with an inner and outer depth ratio of 1:2 and a blunt edge of 2-3 mm. The welding material is a combination of TSW-12KHG submerged arc welding wire and TF-210 submerged arc welding flux from Tiantai Welding Material Manufacturer. After welding, the steel plate is slowly cooled and kept warm, and the interlayer temperature is controlled below 200°C.

[0070] (4) The outer surface of the steel pipe is shot peened and the anti-corrosion coating is prepared in sequence. The pressure of the shot peening is 0.5 MPa and the time is 10 min. The anti-corrosion coating for preparing the anti-corrosion coating includes the following raw materials in parts by weight: 50 parts of phenolic epoxy resin F-51, 35 parts of kaolin, 10 parts of active diluent, 3 parts of dispersant BYK-163, 0.5 parts of polyether defoamer AM1512, 20 parts of 1-(2-hydroxyethyl)-5-aminopyrazole, and the curing conditions are 25°C / 24h.

[0071] Example 5

[0072] (1) Same as Example 1.

[0073] (2) The steel plate is rolled into a round shape by cold rolling, and the wall thickness of the steel plate is 150 mm.

[0074] (3) The steel plate is preheated before welding to a temperature of 123°C. The single-wire submerged arc welding process is adopted. The welding groove is a double-sided X-shaped groove with an inner and outer depth ratio of 1:2 and a blunt edge of 2-3 mm. The welding material is a combination of TSW-12KHG submerged arc welding wire and TF-210 submerged arc welding flux from Tiantai Welding Material Manufacturer. After welding, the steel plate is slowly cooled and kept warm, and the interlayer temperature is controlled below 200°C.

[0075] (4) The outer surface of the steel pipe is shot peened and the anti-corrosion coating is prepared in sequence. The pressure of the shot peening is 0.6 MPa and the time is 10 min. The anti-corrosion coating for preparing the anti-corrosion coating includes the following raw materials in parts by weight: 45 parts of phenolic epoxy resin F-44, 30 parts of wollastonite powder, 8 parts of active diluent, 3 parts of dispersant BYK-163, 0.3 parts of polyether defoamer AM1512, 15 parts of 1-(2-hydroxyethyl)-5-aminopyrazole, and the curing conditions are 25°C / 24h.

[0076] Example 6

[0077] (1) Same as Example 1.

[0078] (2) The steel plate is rolled into a round shape by cold rolling, and the wall thickness of the steel plate is 150 mm.

[0079] (3) The steel plate is preheated before welding to a temperature of 123°C. The single-wire submerged arc welding process is adopted. The welding groove is a double-sided X-shaped groove with an inner and outer depth ratio of 1:2 and a blunt edge of 2-3 mm. The welding material is a combination of TSW-12KHG submerged arc welding wire and TF-210 submerged arc welding flux from Tiantai Welding Material Manufacturer. After welding, the steel plate is slowly cooled and kept warm, and the interlayer temperature is controlled below 200°C.

[0080] (4) The outer surface of the steel pipe is shot peened and the anti-corrosion coating is prepared in sequence. The pressure of the shot peening is 0.8 MPa and the time is 5 min. The anti-corrosion coating for preparing the anti-corrosion coating includes the following raw materials in parts by weight: 40 parts of phenolic epoxy resin F-51, 25 parts of mica powder, 5 parts of active diluent, 32 parts of dispersant BYK-16, 0.2 parts of polyether defoamer AM1512, 10 parts of 1-(2-hydroxyethyl)-5-aminopyrazole, and the curing conditions are 25°C / 24h.

[0081] Comparative Example 1

[0082] The preparation method of the steel pipe is the same as that of Example 1, except that the 1-(2-hydroxyethyl)-5-aminopyrazole in Example 1 is replaced by the same weight portion of diethylenetriamine, and the curing condition is 25° C. / 24 h.

[0083] Comparative Example 2

[0084] The preparation method of the steel pipe is the same as that of Example 1, except that the 1-(2-hydroxyethyl)-5-aminopyrazole in Example 1 is replaced by the same weight portion of m-phenylenediamine, and the curing conditions are 60° C. / 2h+150° C. / 2h.

[0085] Comparative Example 3

[0086] The preparation method of the steel pipe is the same as that of Example 1, except that the 1-(2-hydroxyethyl)-5-aminopyrazole in Example 1 is replaced by the same weight portion of polyamide 650, and the curing condition is 25° C. / 24 h.

[0087] Comparative Example 4

[0088] The preparation method of the steel pipe is the same as that of Example 1, except that the 1-(2-hydroxyethyl)-5-aminopyrazole in Example 1 is replaced by 35 parts of diethylenetriamine, and the curing conditions are 25° C. / 24 h.

[0089] Comparative Example 5

[0090] The preparation method of the steel pipe is the same as that of Example 1, except that the 1-(2-hydroxyethyl)-5-aminopyrazole in Example 1 is replaced by 35 parts of m-phenylenediamine, and the curing conditions are 60° C. / 2h+150° C. / 2h.

[0091] Comparative Example 6

[0092] The preparation method of the steel pipe is the same as that of Example 1, except that the 1-(2-hydroxyethyl)-5-aminopyrazole in Example 1 is replaced by 35 parts of polyamide 650, and the curing conditions are 25° C. / 24 h.

[0093] The performance of the anti-corrosion coatings prepared in the above Examples 4-5 and Comparative Examples 1-6 was tested, and the test results are shown in Table 4.

[0094] The salt water resistance of the anti-corrosion coating was tested according to GB10834-1989.

[0095] Table 4

[0096]

[0097]

[0098] As can be seen from Table 4, under the same dosage conditions, compared with diethylenetriamine, m-phenylenediamine, and polyamide 650 commonly used in the art, the present invention uses 1-(2-hydroxyethyl)-5-aminopyrazole as a curing agent to significantly improve the salt water resistance of the coating, and even if the dosage of diethylenetriamine, m-phenylenediamine, and polyamide 650 is greatly increased, the coating cannot achieve salt water resistance comparable to that of 1-(2-hydroxyethyl)-5-aminopyrazole. In other words, the present invention uses 1-(2-hydroxyethyl)-5-aminopyrazole as a curing agent to not only achieve the curing of epoxy resin, but also improve the salt water resistance of the coating.

[0099] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing an ultra-thickness longitudinal submerged arc welded steel pipe, characterized in that: The preparation method comprises the following steps: (1) Confirmation of chemical composition and properties of steel plates; (2) Rolling the steel plate; (3) Preheat the steel plate before welding, adopt submerged arc welding technology, the welding groove is a double-sided X-shaped groove, slow cooling and insulation after welding, and the interlayer temperature is controlled below 200℃.

2. The preparation method according to claim 1, characterized in that: The steel plate includes the following components in mass percentage: Mn 1.32-1.60%, Si 0.15-0.48%, Ni 0.20-0.75%, Cr 0.06-0.25%, C 0.07-0.12%, Cu 0.03-0.19%, Mo 0.01-0.05%, Alt 0.02-0.06%, Nb 0.016-0.03%, Ti 0.007-0.02%, V 0.002-0.022%, P≤0.019%, N≤0.0062%, S≤0.006%, Ceq0.41-0.42%, Pcm0.18-0.23%, and the balance is Fe and unavoidable impurities.

3. The preparation method according to claim 1, characterized in that: The steel plate rolling method includes hot rolling method, cold rolling method and mechanical rolling method.

4. The preparation method according to claim 1, characterized in that: The preheating temperature of the steel plate before welding is in the range of 120-150°C.

5. The preparation method according to claim 1, characterized in that: The inner and outer depth ratio of the welding groove is 1:2, and the blunt edge is 2-3 mm.

6. The preparation method according to claim 1, characterized in that: The submerged arc welding is single-wire submerged arc welding.

7. The preparation method according to claim 1, characterized in that: The submerged arc welding uses low-Ni alloy welding wire and fluorine-alkali type flux.

8. An ultra-thickness straight seam submerged arc welded steel pipe prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Method of submerged-arc welding of thick sheet S355NL for low-temperature wind tower

    CN101862887A

  • Thick plate submerged arc welding technology for low-temperature maritime engineering

    CN102363238A

  • High-temperature-resistant and high-pressure-resistant high-alloy submerged arc welded steel pipe welding process

    CN109454316A

  • Large-caliber longitudinal submerged arc welded steel pipe welding technology for offshore wind power

    CN109530855A

  • Preparation process of longitudinal submerged arc welded steel pipe for offshore wind power jacket foundation

    CN112620876A