Graded pore structure g-C3N4 / TiO2 as well as preparation method and application thereof
By forming a hierarchical pore structure on g-C3N4 and uniformly loading TiO2 nanoparticles, the problem of uneven TiO2 loading in the existing technology is solved, and the catalytic performance and hydrogen absorption and release effect of solid hydrogen storage materials are significantly improved.
Patent Information
- Application Number
- CN202410794497.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult to achieve uniform loading of TiO2 on the surface and inside of titanium nitride in solid hydrogen storage materials with existing technology, resulting in poor catalytic modification effect.
The hierarchical pore structure g-C3N4/TiO2 composite material is used. The hierarchical pore structure is formed by mixing, calcining and etching monodisperse SiO2 balls and amino compounds, and then evenly loading TiO2 nanoparticles through hydrothermal reaction, combined with ball milling mixing to improve catalytic performance. .
The hierarchical pore structure of the g-C3N4/TiO2 composite material was achieved, which improved the catalytic performance and catalytic hydrogen absorption and release effect, and significantly improved the modification performance of the solid hydrogen storage material.
Smart Images

Figure HDA0004901063880000011 
Figure HDA0004901063880000012 
Figure HDA0004901063880000021
Abstract
Description
Technical Field
[0001] The present invention relates to the field of nano material preparation, and in particular to a hierarchical pore structure gC 3 N 4 / TiO 2 And its preparation method and application. Background Art
[0002] C 3 N 4 It is a covalent compound composed of carbon atoms and nitrogen atoms. It is a typical n-type semiconductor with high chemical stability, thermal stability, carrier migration and other capabilities. Therefore, it has a very broad application prospect, especially in the field of catalysis. For catalytic materials, specific surface area is a very important structural parameter. Improving gC 3 N 4 The specific surface area has a significant effect on the improvement of carrier transport and the number of active sites.
[0003] The most important method to increase the specific surface area is to synthesize porous gC 3 N 4 Morphology. Currently commonly used porous gC 3 N 4 The synthesis method is the template method, which includes the soft template method and the hard template method. The soft template method mainly uses surfactants or polymers as precursors to achieve material self-assembly and template removal under high temperature conditions. However, the gC synthesized by this method is 3 N 4 The porosity is low and the structure is difficult to control. The hard template method uses self-sacrificial particles of different shapes and sizes to effectively control gC 3 N 4 In the hard template method, the selection of template type, the chemical ratio of template agent and precursor all have an impact on gC 3 N 4 The pore size and porosity have a very important influence.
[0004] Based on porous gC 3 N 4 Due to its excellent structure and catalytic performance, it has been widely used and developed in the energy field. For example, it can be used as a carrier to load various metal or metal oxide particles, thereby improving the dispersion of catalyst particles and achieving a synergistic catalytic effect. Transition metals such as Ti, Ni, and Co have excellent catalytic modification effects due to their unique outer electron configuration. Loading them on porous gC 3 N 4The composite material is obtained in the pores of the material, which has very important application value in the energy field, especially in the field of solid hydrogen storage. For example, Chinese patent document CN116768151A discloses a graphite phase carbon nitride-based titanium dioxide doped lithium aluminum hydride hydrogen storage material, which uses dicyandiamide and titanyl sulfate as raw materials, dicyandiamide as carbon source and nitrogen source, and titanyl sulfate as titanium source; after grinding and mixing, calcination is performed, and then TiO 2 @gC 3 N 4 The doping amount is 3-10wt% and ball milled with lithium aluminum hydride; wherein gC 3 N 4 The microstructure of TiO 2 The microstructure of TiO 2 The particle size of the nanoparticles is 8-9nm, TiO 2 @gC 3 N 4 The microstructure of TiO 2 Uniform load at gC 3 N 4 surface. It can be applied to hydrogen storage materials. However, the titanium nitride synthesized by this method has small porosity and small pore size, making it difficult to achieve TiO 2 Even after ball milling, it is difficult to achieve uniform dispersion of the titanium nitride on the surface and inside of the titanium nitride in the solid hydrogen storage material, which is not conducive to improving the catalytic modification effect. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a hierarchical pore structure gC 3 N 4 / TiO 2 And its preparation method and application. The preparation method of the present invention is simple, and the obtained gC 3 N 4 / TiO 2 For porous gC 3 N 4 Uniformly load TiO on the surface or in the pores 2 Nanoparticles have a hierarchical pore structure, a high specific surface area and a high porosity; the hierarchical pore structure gC 3 N 4 / TiO 2 Applied in the field of solid hydrogen storage, gC 3 N 4 and TiO 2 A synergistic effect will be produced, and combined with the hierarchical pore structure, it will show excellent solid-state hydrogen storage modified catalytic performance.
[0006] The technical solution of the present invention is as follows:
[0007] A hierarchical pore structure gC3 N 4 / TiO 2 , the gC 3 N 4 / TiO 2 gC is a hierarchical pore structure 3 N 4 Uniformly load TiO on the surface or in the pores 2 Nanoparticles.
[0008] According to the preferred embodiment of the present invention, gC 3 N 4 / TiO 2 The pore size is 50-100nm, TiO 2 The particle size of nanoparticles is 100-200nm.
[0009] The above hierarchical pore structure gC 3 N 4 / TiO 2 The preparation method comprises the steps of:
[0010] (1) Monodispersed SiO 2 The balls are fully mixed with the amino compound and calcined to obtain gC 3 N 4 / SiO 2 ; Then the SiO is removed by etching 2 Get the hierarchical pore structure gC 3 N 4 ;
[0011] (2) Titanium tetrachloride, deionized water, ethylene glycol, hierarchical pore structure gC 3 N 4 The mixture is fully mixed and dispersed uniformly, and then filtered, washed and dried to obtain the hierarchical pore structure gC. 3 N 4 / TiO 2 .
[0012] According to the preferred embodiment of the present invention, in step (1), monodispersed SiO 2 The preparation method of the ball comprises the steps of: mixing anhydrous ethanol, deionized water and concentrated ammonia water uniformly, adding tetraethyl orthosilicate dropwise, reacting, centrifuging, washing and drying to obtain monodispersed SiO 2 ball.
[0013] Preferably, the mass concentration of concentrated ammonia water is 25% to 28%; the volume ratio of anhydrous ethanol to deionized water is (6 to 10):1; the volume ratio of deionized water to concentrated ammonia water is (2 to 3):1; the volume ratio of tetraethyl orthosilicate to deionized water is (0.3 to 0.5):1.
[0014] Preferably, the reaction temperature is 40-50°C and the reaction time is 1-2h. Tetraethyl orthosilicate undergoes hydrolysis under alkaline conditions provided by ammonia water to generate monodisperse SiO 2 The appropriate reaction temperature can provide a stable environment and regulate the hydrolysis rate of tetraethyl orthosilicate and the SiO 2 The sphere formation rate can form monodispersed SiO 2 If the reaction temperature is not appropriate, the SiO 2 The diameter of the spherical particles is not uniform.
[0015] Preferably according to the present invention, in step (1), the amino compound is one or a combination of two or more of urea, biuret, dicyandiamide or melamine.
[0016] According to the preferred embodiment of the present invention, in step (1), monodispersed SiO 2 The mass ratio of the spheres to the amino compound is (0.025-3):1, preferably (0.2-3):1. Suitable monodispersed SiO 2 The mass ratio of spheres to amino compounds can adjust gC 3 N 4 The number and size of graded pores on the surface form a graded pore structure with controllable pore size and porosity. 2 If the proportion of balls is too small, then gC 3 N 4 The number of pores formed on the surface is small, and it is impossible to form a hierarchical pore structure. 2 If the proportion of spheres is too high, the number of pores will be too high and cause the collapse of the entire framework structure. Therefore, the appropriate monodisperse SiO 2 The mass ratio of spheres to amino compounds is very important for the formation of the hierarchical pore structure, which in turn affects the catalytic performance of the resulting materials.
[0017] Preferably, according to the present invention, in step (1), the calcination temperature is 550-600° C., the calcination time is 2-4 hours, and the calcination atmosphere is an inert gas; preferably, the inert gas is nitrogen or argon.
[0018] According to the preferred embodiment of the present invention, in step (1), the etching method comprises the steps of: 3 N 4 / SiO 2 Immerse in the corrosive solution, undergo etching reaction, filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 .
[0019] Preferably, the etching solution is one of a hydrofluoric acid aqueous solution or an ammonium bifluoride aqueous solution, and the concentration of the etching solution is (2-5) mol / L. Within this concentration range, monodisperse SiO 2 balls and maintain the integrity of the graded pore structure.
[0020] Preferably, monodisperse SiO 2 The ratio of the mass of the ball to the volume of the corrosive liquid is 1: (4-200) g / mL.
[0021] Preferably, the etching reaction temperature is room temperature, the etching reaction is carried out under stirring conditions, and the etching reaction time is 12-24 hours.
[0022] According to the preferred embodiment of the present invention, in step (2), the volume ratio of titanium tetrachloride, deionized water and ethylene glycol is 1:(0.8-1.5):(25-45); titanium tetrachloride and the hierarchical pore structure gC 3 N 4 The mass ratio of ethylene glycol is (0.9-3.3):1. The appropriate content of ethylene glycol can help the nano-titanium dioxide particles formed by the hydrolysis of titanium tetrachloride to suspend and form a sol, improve the dispersibility of the nano-particles in the liquid, and then improve the uniformity of the particle size. Too low or too high a proportion of ethylene glycol will reduce the uniformity of TiO 2 The uniformity of particle size affects the catalytic performance of the obtained material. At the same time, suitable titanium tetrachloride and hierarchical pore structure gC 3 N 4 The mass ratio can ensure that TiO 2 Particles in hierarchical pore structure gC 3 N 4 The uniform loading on the surface, if the proportion of titanium tetrachloride is too high, the excess TiO 2 Particles will block the hierarchical pore structure and reduce the TiO 2 Particles in gC 3 N 4 The uniformity of surface distribution reduces the catalytic performance of the resulting material.
[0023] According to the preferred embodiment of the present invention, in step (2), the hydrothermal reaction temperature is 150-180°C and the hydrothermal reaction time is 4-8h. Within this temperature range, titanium tetrachloride is hydrolyzed to generate TiO 2 Particles and attached to the hierarchical pore structure gC 3 N 4 On the surface and in the pores, gC is formed 3 N 4 / TiO 2 Composite materials.
[0024] The above hierarchical pore structure gC 3 N 4 / TiO2 Application in hydrogen storage.
[0025] According to a preferred embodiment of the present invention, the application method comprises the steps of: 3 N 4 / TiO 2 The composite material is uniformly mixed with magnesium hydride by ball milling to be used for hydrogen storage.
[0026] Preferably, the hierarchical pore structure gC 3 N 4 / TiO 2 The mass ratio of magnesium hydride to magnesium hydride is 1:5-15; the ball milling speed is 200-600r / min, and the ball milling time is 1-3h.
[0027] The technical features and beneficial effects of the present invention are as follows:
[0028] (1) Tetraethyl orthosilicate hydrolyzes under alkaline conditions to generate monodisperse SiO 2 Amide compounds will decompose to form gC under high temperature calcination conditions. 3 N 4 , monodisperse SiO 2 The ball is loaded on gC 3 N 4 Composite material gC 3 N 4 / SiO 2 . gC 3 N 4 / SiO 2 After etching, the monodisperse SiO 2 ball, and in gC 3 N 4 A large number of pores are left in the porous material to form a porous material with a hierarchical pore structure. 3 N 4 . gC 3 N 4 After mixing with titanium tetrachloride, deionized water and ethylene glycol, titanium tetrachloride is hydrolyzed under solvent thermal conditions to generate TiO 2 , and loaded on gC 3 N 4 The surface and pores of gC 3 N 4 / TiO 2 Composite material. The hierarchical pore structure of the present invention gC 3 N 4 / TiO 2 The synthesis method is simple. By using simple liquid phase reaction, calcination, etching and solvent thermal reaction, gC with hierarchical pore structure can be prepared. 3 N 4 / TiO2 .
[0029] (2) gC obtained by the present invention 3 N 4 / TiO 2 gC is the hierarchical pore structure 3 N 4 TiO is loaded on the surface or in the pores 2 Nanoparticles (particle size 100-200nm), with hierarchical pore structure (pore size 50-100nm), high specific surface area and porosity, TiO 2 The uniform distribution of nanoparticles is beneficial to improving catalytic performance.
[0030] (3) gC obtained by the present invention 3 N 4 / TiO 2 In, gC 3 N 4 The shared electron pair formed by the CN bond in TiO 2 The multivalent Ti in gC can provide active sites for the transfer of H. 3 N 4 / TiO 2 Through synergistic effect, the catalytic performance of hydrogen storage material modification is improved. As a whole, the preparation method of the present invention, each step and each condition work together to obtain the hierarchical pore structure gC of the structure and performance of the present invention. 3 N 4 / TiO 2 The hierarchical pore structure of the present invention gC 3 N 4 / TiO 2 Applied in the field of solid hydrogen storage, due to gC 3 N 4 and TiO 2 The synergistic effect, combined with the hierarchical pore structure, enhances the catalytic hydrogen absorption and desorption effect of the material, showing excellent solid-state hydrogen storage modified catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The hierarchical pore structure gC prepared in Example 1 3 N 4 / TiO 2 SEM images of
[0032] Figure 2 gC prepared in Example 1 3 N 4 / TiO 2 XRD pattern of modified magnesium hydride;
[0033] Figure 3 gC prepared in Example 1 3 N 4 / TiO 2 SEM and element distribution of modified magnesium hydride;
[0034] Figure 4 The hierarchical pore structure gC prepared in Example 2 3 N 4 / TiO 2 XRD pattern of
[0035] Figure 5 The hierarchical pore structure gC prepared in Example 3 3 N 4 / TiO 2 XPS graphs of (a) C 1s; (b) N 1s; (c) Ti2p;
[0036] Figure 6 gC prepared in Example 3 3 N 4 / TiO 2 Temperature-dependent hydrogen release curves of modified magnesium hydride and unmodified magnesium hydride;
[0037] Figure 7 Preparation of gC for Example 4 3 N 4 / TiO 2 Isothermal hydrogen absorption curves of modified magnesium hydride and unmodified magnesium hydride;
[0038] Figure 8 The hierarchical pore structure gC prepared in Example 5 3 N 4 / TiO 2 SEM images of
[0039] Fig. 9 gC prepared in Example 6 3 N 4 / TiO 2 SEM image of modified magnesium hydride;
[0040] Fig.10 The hierarchical pore structure gC prepared in Comparative Example 1 3 N 4 SEM images of
[0041] Fig.11 The hierarchical pore structure gC prepared in Comparative Example 1 3 N 4 Temperature-dependent hydrogen release curves of modified magnesium hydride and unmodified magnesium hydride;
[0042] Fig.12 The hierarchical pore structure gC prepared in Comparative Example 23 N 4 / TiO 2 SEM image of . DETAILED DESCRIPTION
[0043] The present invention is further described below with reference to specific embodiments, but is not limited thereto.
[0044] Meanwhile, the experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0045] Example 1
[0046] A hierarchical pore structure gC 3 N 4 / TiO 2 The preparation method comprises the steps of:
[0047] (1) 150 mL of anhydrous ethanol, 15 mL of deionized water and 6 mL of concentrated ammonia with a mass concentration of 25% were mixed and heated in a water bath at 40°C. 6 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued under constant temperature water bath stirring for 1 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained after washing and drying. 2 ball;
[0048] (2) 0.4 g of monodispersed SiO 2 The balls were mixed evenly with 2g of melamine and calcined at 550℃ for 3h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2 Immerse in 8mL2 mol / L hydrofluoric acid aqueous solution, etch and stir at room temperature for 12h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0049] (3) 1 mL of titanium tetrachloride and 1 mL of deionized water were added to 30 mL of ethylene glycol, stirred and mixed, and after the solution was clarified, 0.8 g of hierarchical pore structure gC was added 3 N 4 , continue to stir and mix evenly, then transfer the mixed solution into a reactor, keep it at 160℃ for 4h, and then filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 / TiO 2 Composite materials.
[0050] like Figure 1 The gC prepared in this example is shown. 3 N 4 / TiO 2 The SEM image of the composite material shows that C 3 N 4 There is a hierarchical porous structure in the surface, and TiO is evenly loaded on the surface. 2 Nanoparticles. Pore size is 50-100nm, TiO 2 The particle size is 100-200nm.
[0051] 0.1 g gC 3 N 4 / TiO 2 The mixture was ball-milled with 0.9 g of commercial magnesium hydride at a speed of 400 r / min for 2 h to obtain a composite material, namely gC 3 N 4 / TiO 2 Modified magnesium hydride.
[0052] like Figure 2 Shown is gC prepared in Example 1 3 N 4 / TiO 2 XRD diagram of modified magnesium hydride. It can be seen from the figure that C 3 N 4 、TiO 2 MgH 2 There are obvious diffraction peaks, and no diffraction peaks of other phases exist, which proves that the gC synthesized by this method 3 N 4 / TiO 2 The composite material of modified magnesium hydride has higher purity.
[0053] like Figure 3 Shown is gC prepared in Example 1 3 N 4 / TiO 2 SEM and element distribution diagram of modified magnesium hydride. It can be seen from the figure that C, N, O, Mg, and Ti elements are evenly dispersed, proving that the gC synthesized by this method is 3 N 4 / TiO 2 Evenly dispersed in MgH 2 In the matrix, this is beneficial to improve its catalytic modification effect.
[0054] The composite material (gC 3 N 4 / TiO 2Modified magnesium hydride) was tested for hydrogen desorption and absorption performance. The hydrogen desorption performance test was as follows: 200 mg of the composite material was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500°C at a heating rate of 5°C / min. The amount of hydrogen released during this process was measured and plotted as a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200 mg of the composite material was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250°C at a heating rate of 5°C / min. A hydrogen pressure of 5MPa was provided at 250°C and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and plotted as an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and absorption performance under the same conditions, and the obtained performance was compared with that of gC 3 N 4 / TiO 2 The modified samples were compared.
[0055] After testing, gC 3 N 4 / TiO 2 Catalytically modified magnesium hydride can significantly reduce the dehydrogenation temperature and increase the dehydrogenation and absorption capacity. The initial dehydrogenation temperature and peak dehydrogenation temperature of unmodified magnesium hydride are 317°C and 375°C, and the dehydrogenation rate is 93.1%. 3 N 4 / TiO 2 After modification, the initial dehydrogenation temperature and peak dehydrogenation temperature were reduced to 197℃ and 318℃, respectively, and the dehydrogenation rate was 95.6%. After 1.5h of hydrogen absorption, the hydrogen absorption of unmodified magnesium hydride was only 4.12wt.%, reaching only 54.2% of the hydrogen absorption rate, while gC 3 N 4 / TiO 2 The hydrogen absorption capacity of the catalytically modified magnesium hydride is 6.54wt.%, reaching a hydrogen absorption rate of 95.6%, which is a significant improvement.
[0056] Example 2
[0057] A hierarchical pore structure gC 3 N 4 / TiO 2 The preparation method comprises the steps of:
[0058] (1) 120 mL of anhydrous ethanol, 20 mL of deionized water, and 8 mL of concentrated ammonia with a mass concentration of 26% were mixed and heated in a water bath at 40°C. 7 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued under constant temperature water bath stirring for 2 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained after washing and drying. 2 ball;
[0059] (2) 0.5 g monodispersed SiO 2The balls were mixed evenly with 1 g of urea and calcined at 560 °C for 4 h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2 Immerse in 9mL4 mol / L hydrogen fluoride ammonium aqueous solution, etch and stir at room temperature for 16h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0060] (3) 1.5 mL of titanium tetrachloride and 2 mL of deionized water were added to 38 mL of ethylene glycol, stirred and mixed, and after the solution was clarified, 0.8 g of hierarchical pore structure gC was added. 3 N 4 , continue to stir and mix evenly, then transfer the mixed solution into a reactor, keep it at 165℃ for 5h, and then filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 / TiO 2 Composite materials.
[0061] like Figure 4 The gC prepared in this example is shown. 3 N 4 / TiO 2 The XRD diagram of the composite material shows that the C 3 N 4 and TiO 2 The diffraction peaks indicate the formation of these two phases with high purity.
[0062] 0.1 g gC 3 N 4 / TiO 2 It was ball-milled with 0.9g of commercial magnesium hydride at a speed of 400r / min and a ball-milling time of 2h. The obtained composite sample was tested for hydrogen desorption and hydrogen absorption. The hydrogen desorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500℃ at a heating rate of 5℃ / min. The amount of hydrogen released during this process was measured and drawn into a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250℃ at a heating rate of 5℃ / min. A hydrogen pressure of 5MPa was provided at 250℃ and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and drawn into an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and hydrogen absorption performance under the same conditions, and the obtained performance was compared with gC 3 N4 / TiO 2 The modified samples were compared.
[0063] After testing, gC 3 N 4 / TiO 2 Catalytically modified magnesium hydride can significantly reduce the dehydrogenation temperature and increase the dehydrogenation and absorption capacity. The initial dehydrogenation temperature and peak dehydrogenation temperature of unmodified magnesium hydride are 317°C and 375°C, and the dehydrogenation rate is 93.1%. 3 N 4 / TiO 2 After modification, the initial dehydrogenation temperature and peak dehydrogenation temperature were reduced to 208℃ and 325℃, respectively, and the dehydrogenation rate was 94.1%. After 1.5h of hydrogen absorption, the hydrogen absorption of unmodified magnesium hydride was only 4.12wt.%, reaching only 54.2% of the hydrogen absorption rate, while gC 3 N 4 / TiO 2 The hydrogen absorption capacity of the catalytically modified magnesium hydride is 6.42wt.%, reaching a hydrogen absorption rate of 93.8%, which is a significant improvement.
[0064] Example 3
[0065] A hierarchical pore structure gC 3 N 4 / TiO 2 The preparation method comprises the steps of:
[0066] (1) 210 mL of anhydrous ethanol, 30 mL of deionized water and 12 mL of concentrated ammonia with a mass concentration of 25% were mixed and heated in a water bath at 45°C. 10 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued in a constant temperature water bath with stirring for 1.5 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained by washing and drying. 2 ball;
[0067] (2) 1.5 g monodispersed SiO 2 The balls were mixed evenly with 0.5 g of urea and calcined at 580 °C for 3.5 h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2 Immerse in 20mL5 mol / L hydrogen fluoride ammonium aqueous solution, etch and stir at room temperature for 18h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0068] (3) 2 mL of titanium tetrachloride and 2 mL of deionized water were added to 50 mL of ethylene glycol, stirred and mixed, and after the solution was clarified, 3.5 g of hierarchical pore structure gC was added. 3 N 4 , continue to stir and mix evenly, then transfer the mixed solution into a reactor, keep it at 160℃ for 5h, and then filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 / TiO 2 Composite materials.
[0069] like Figure 5 The hierarchical pore structure gC prepared in this example is shown 3 N 4 / TiO 2 XPS graph shows the combined valence states of C, N, and Ti, proving that gC 3 N 4 / TiO 2 The formation of physical phases.
[0070] 0.1 g gC 3 N 4 / TiO 2 It was ball-milled with 0.9g of commercial magnesium hydride at a speed of 400r / min and a ball-milling time of 2h. The obtained composite sample was tested for hydrogen desorption and hydrogen absorption. The hydrogen desorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500℃ at a heating rate of 5℃ / min. The amount of hydrogen released during this process was measured and drawn into a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250℃ at a heating rate of 5℃ / min. A hydrogen pressure of 5MPa was provided at 250℃ and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and drawn into an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and hydrogen absorption performance under the same conditions, and the obtained performance was compared with gC 3 N 4 / TiO 2 The modified samples were compared.
[0071] After testing, gC 3 N 4 / TiO 2 Catalytically modified magnesium hydride can significantly reduce the dehydrogenation temperature and increase the dehydrogenation and absorption capacity (such as Figure 6 The initial and peak dehydrogenation temperatures of unmodified magnesium hydride are 317°C and 375°C, respectively, and the dehydrogenation rate is 93.1%. 3 N 4 / TiO2 After modification, the initial dehydrogenation temperature and peak dehydrogenation temperature were reduced to 212℃ and 330℃, respectively, and the dehydrogenation rate was 93.3%. After 1.5h of hydrogen absorption, the hydrogen absorption of unmodified magnesium hydride was only 4.12wt.%, reaching only 54.2% of the hydrogen absorption rate, while gC 3 N 4 / TiO 2 The hydrogen absorption capacity of the catalytically modified magnesium hydride is 6.40wt.%, reaching a hydrogen absorption rate of 93.6%, which is a significant improvement.
[0072] Example 4
[0073] A hierarchical pore structure gC 3 N 4 / TiO 2 The preparation method comprises the steps of:
[0074] (1) 180 mL of anhydrous ethanol, 20 mL of deionized water and 8 mL of concentrated ammonia with a mass concentration of 26% were mixed and heated in a water bath at 45°C. 9 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued under constant temperature water bath stirring for 1 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained after washing and drying. 2 ball;
[0075] (2) 2g monodispersed SiO 2 The balls were mixed evenly with 1g of dicyandiamide and calcined at 570℃ for 4h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2 Immerse in 30mL 3 mol / L hydrofluoric acid aqueous solution, etch and stir at room temperature for 20h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0076] (3) 3 mL of titanium tetrachloride and 4 mL of deionized water were added to 80 mL of ethylene glycol, stirred and mixed, and after the solution was clarified, 4.3 g of hierarchical pore structure gC was added. 3 N 4 , continue to stir and mix evenly, then transfer the mixed solution into a reactor, keep it at 170℃ for 4h, and then filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 / TiO 2 Composite materials.
[0077] 0.1 g gC 3 N 4 / TiO 2 It was ball-milled with 0.9g of commercial magnesium hydride at a speed of 400r / min and a ball-milling time of 2h. The obtained composite sample was tested for hydrogen desorption and hydrogen absorption. The hydrogen desorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500℃ at a heating rate of 5℃ / min. The amount of hydrogen released during this process was measured and drawn into a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250℃ at a heating rate of 5℃ / min. A hydrogen pressure of 5MPa was provided at 250℃ and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and drawn into an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and hydrogen absorption performance under the same conditions, and the obtained performance was compared with gC 3 N 4 / TiO 2 The modified samples were compared.
[0078] After testing, gC 3 N 4 / TiO 2 Catalytically modified magnesium hydride can significantly reduce the dehydrogenation temperature and increase the dehydrogenation and absorption capacity. The initial dehydrogenation temperature and peak dehydrogenation temperature of unmodified magnesium hydride are 317°C and 375°C, and the dehydrogenation rate is 93.1%. 3 N 4 / TiO 2 After modification, the initial dehydrogenation temperature and peak dehydrogenation temperature were reduced to 215℃ and 328℃, respectively, and the dehydrogenation rate was 93.2%. Figure 7 As shown in Figure 2, after 1.5 h of hydrogen absorption, the hydrogen absorption capacity of the unmodified magnesium hydride was only 4.12 wt.%, reaching only 54.2% of the hydrogen absorption rate, while gC 3 N 4 / TiO 2 The hydrogen absorption capacity of the catalytically modified magnesium hydride is 6.37wt.%, reaching a hydrogen absorption rate of 93.1%, which is a significant improvement.
[0079] Example 5
[0080] A hierarchical pore structure gC 3 N 4 The preparation method comprises the steps of:
[0081] (1) 150 mL of anhydrous ethanol, 15 mL of deionized water and 6 mL of concentrated ammonia with a mass concentration of 25% were mixed and heated in a water bath at 40°C. 6 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued under constant temperature water bath stirring for 1 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained after washing and drying. 2 ball;
[0082] (2) 0.4 g of monodispersed SiO 2 The balls were mixed evenly with 2g of melamine and calcined at 550℃ for 3h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2 Immerse in 8mL2 mol / L hydrofluoric acid aqueous solution, etch and stir at room temperature for 12h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0083] (3) 1.2 mL of titanium tetrachloride and 1 mL of deionized water were added to 30 mL of ethylene glycol, stirred and mixed, and after the solution was clarified, 0.8 g of hierarchical pore structure gC was added. 3 N 4 , continue to stir and mix evenly, then transfer the mixed solution into a reactor, keep it at 160℃ for 4h, and then filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 / TiO 2 Composite materials.
[0084] like Figure 8 The gC prepared in this example is shown. 3 N 4 / TiO 2 The SEM image of the composite material shows that C 3 N 4 There is a hierarchical porous structure in the surface, and TiO is evenly loaded on the surface. 2 Nanoparticles. As the amount of titanium tetrachloride added increases, C 3 N 4 Surface TiO 2 The number and size of nanoparticles increased (compared to Figure 1 ).
[0085] 0.1 g gC 3 N 4 / TiO 2It was ball-milled with 0.9g of commercial magnesium hydride at a speed of 400r / min and a ball-milling time of 2h. The obtained composite sample was tested for hydrogen desorption and hydrogen absorption. The hydrogen desorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500℃ at a heating rate of 5℃ / min. The amount of hydrogen released during this process was measured and drawn into a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250℃ at a heating rate of 5℃ / min. A hydrogen pressure of 5MPa was provided at 250℃ and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and drawn into an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and hydrogen absorption performance under the same conditions, and the obtained performance was compared with gC 3 N 4 / TiO 2 The modified samples were compared.
[0086] After testing, gC 3 N 4 / TiO 2 Catalytically modified magnesium hydride can significantly reduce the dehydrogenation temperature and increase the dehydrogenation and absorption capacity. The initial dehydrogenation temperature and peak dehydrogenation temperature of unmodified magnesium hydride are 317°C and 375°C, and the dehydrogenation rate is 93.1%. 3 N 4 / TiO 2 After modification, the initial dehydrogenation temperature and peak dehydrogenation temperature were reduced to 211℃ and 327℃, respectively, and the dehydrogenation rate was 93.5%. After 1.5h of hydrogen absorption, the hydrogen absorption of unmodified magnesium hydride was only 4.12wt.%, reaching only 54.2% of the hydrogen absorption rate, while gC 3 N 4 / TiO 2 The hydrogen absorption capacity of the catalytically modified magnesium hydride is 6.41wt.%, reaching a hydrogen absorption rate of 93.7%, which is a significant improvement.
[0087] Example 6
[0088] A hierarchical pore structure gC 3 N 4 / TiO 2 The preparation method comprises the steps of:
[0089] (1) 150 mL of anhydrous ethanol, 15 mL of deionized water and 6 mL of concentrated ammonia with a mass concentration of 25% were mixed and heated in a water bath at 40°C. 6 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued under constant temperature water bath stirring for 1 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained after washing and drying. 2 ball;
[0090] (2) 0.05 g of monodispersed SiO 2 The balls were mixed evenly with 2g of melamine and calcined at 550℃ for 3h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2 Immerse in 8mL2 mol / L hydrofluoric acid aqueous solution, etch and stir at room temperature for 12h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0091] (3) 1 mL of titanium tetrachloride and 1 mL of deionized water were added to 30 mL of ethylene glycol, stirred and mixed, and after the solution was clarified, 0.8 g of hierarchical pore structure gC was added 3 N 4 , continue to stir and mix evenly, then transfer the mixed solution into a reactor, keep it at 160℃ for 4h, and then filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 / TiO 2 Composite materials.
[0092] 0.1 g gC 3 N 4 / TiO 2 It was ball-milled with 0.9g of commercial magnesium hydride at a speed of 400r / min and a ball-milling time of 2h. The obtained composite sample was tested for hydrogen desorption and hydrogen absorption. The hydrogen desorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500℃ at a heating rate of 5℃ / min. The amount of hydrogen released during this process was measured and drawn into a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250℃ at a heating rate of 5℃ / min. A hydrogen pressure of 5MPa was provided at 250℃ and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and drawn into an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and hydrogen absorption performance under the same conditions, and the obtained performance was compared with gC 3 N 4 / TiO 2 The modified samples were compared.
[0093] like Fig. 9 Shown is gC prepared in Example 6 3 N 4 / TiO 2The SEM image of modified magnesium hydride shows that due to the addition of SiO 2 The proportion of spheres is relatively small, so the synthesized gC 3 N 4 / TiO 2 The porosity is low and it is difficult to observe the existence of a large number of pores (compared to Figure 3 ), which is not conducive to uniform compounding with magnesium hydride, thus reducing the catalytic modification effect.
[0094] After testing, gC 3 N 4 / TiO 2 Catalytically modified magnesium hydride can reduce the dehydrogenation temperature and increase the dehydrogenation and absorption capacity, but the modification effect is worse than that of Example 1. The initial dehydrogenation temperature and peak dehydrogenation temperature of unmodified magnesium hydride are 317°C and 375°C, and the dehydrogenation rate is 93.1%. 3 N 4 / TiO 2 After modification, the initial dehydrogenation temperature and peak dehydrogenation temperature were reduced to 221℃ and 325℃, respectively, and the dehydrogenation rate was 93.5%. After 1.5h of hydrogen absorption, the hydrogen absorption of unmodified magnesium hydride was only 4.12wt.%, reaching only 54.2% of the hydrogen absorption rate, while gC 3 N 4 / TiO 2 The hydrogen absorption capacity of the catalytically modified magnesium hydride is 6.08wt.%, reaching a hydrogen absorption rate of 88.9%.
[0095] Comparative Example 1
[0096] A hierarchical pore structure gC 3 N 4 The preparation method comprises the steps of:
[0097] (1) 180 mL of anhydrous ethanol, 20 mL of deionized water and 8 mL of concentrated ammonia with a mass concentration of 26% were mixed and heated in a water bath at 45°C. 9 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued under constant temperature water bath stirring for 1 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained after washing and drying. 2 ball;
[0098] (2) 2g monodispersed SiO 2 The balls were mixed evenly with 1g of dicyandiamide and calcined at 570℃ for 4h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2Immerse in 30mL 3 mol / L hydrofluoric acid aqueous solution, etch and stir at room temperature for 20h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0099] like Fig.10 As shown, the prepared gC 3 N 4 It has a distinct hierarchical porous structure, which can provide more sites for the loading of nanoparticles. During the synthesis of this material, no titanium tetrachloride was added, so there is no TiO 2 existence.
[0100] 0.1 g gC 3 N 4 It was ball-milled with 0.9g of commercial magnesium hydride at a speed of 400r / min and a ball-milling time of 2h. The obtained composite sample was tested for hydrogen desorption and hydrogen absorption. The hydrogen desorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500℃ at a heating rate of 5℃ / min. The amount of hydrogen released during this process was measured and drawn into a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250℃ at a heating rate of 5℃ / min. A hydrogen pressure of 5MPa was provided at 250℃ and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and drawn into an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and hydrogen absorption performance under the same conditions, and the obtained performance was compared with gC 3 N 4 The modified samples were compared.
[0101] After testing, no TiO was loaded 2 GC 3 N 4 The effect of modifying the hydrogen release and absorption properties of magnesium hydride is not obvious. Fig.11 As shown in the figure, the initial dehydrogenation temperature and peak dehydrogenation temperature of unmodified magnesium hydride are 317℃ and 375℃, and the dehydrogenation rate is 93.1%. 3 N 4 After modification, the initial and peak dehydrogenation temperatures were 325°C and 378°C, respectively, and the dehydrogenation rate was 93.0%. After 1.5 hours of hydrogen absorption, the hydrogen absorption of the unmodified magnesium hydride was only 4.12wt.%, reaching only 54.2% of the hydrogen absorption rate. 3 N 4 The hydrogen absorption amount of the catalytically modified magnesium hydride is 4.21wt.%, which is a hydrogen absorption rate of 61.2%.
[0102] Comparative Example 2
[0103] A hierarchical pore structure gC 3 N 4 / TiO 2 The preparation method comprises the steps of:
[0104] (1) 150 mL of anhydrous ethanol, 15 mL of deionized water and 6 mL of concentrated ammonia with a mass concentration of 25% were mixed and heated in a water bath at 40°C. 6 mL of tetraethyl orthosilicate was added dropwise under stirring, and the reaction was continued under constant temperature water bath stirring for 1 h. After the reaction was completed, the precipitate was collected by centrifugation, and monodispersed SiO was obtained after washing and drying. 2 ball;
[0105] (2) 0.4 g of monodispersed SiO 2 The balls were mixed evenly with 2g of melamine and calcined at 550℃ for 3h under nitrogen atmosphere to obtain gC 3 N 4 / SiO 2 , and then the obtained gC 3 N 4 / SiO 2 Immerse in 8mL2 mol / L hydrofluoric acid aqueous solution, etch and stir at room temperature for 12h to remove SiO 2 After the reaction, the hierarchical pore structure gC was obtained by filtration, washing and drying. 3 N 4 ;
[0106] (3) Add 1 mL of titanium tetrachloride to 31 mL of deionized water, stir and mix, and after the solution becomes clear, add 0.8 g of hierarchical pore structure gC 3 N 4 , continue to stir and mix evenly, then transfer the mixed solution into a reactor, keep it at 160℃ for 4h, and then filter, wash and dry to obtain the hierarchical pore structure gC 3 N 4 / TiO 2 Composite materials.
[0107] like Fig.12 Shown is the gC prepared in this comparative example 3 N 4 / TiO 2 SEM images of the composite materials. Figure 1 In contrast, Fig.12 It can be seen that TiO 2 The particle size is relatively large, about 200-400 nm, and since ethylene glycol is not added as a dispersant in the system, the particles are severely agglomerated, which in turn affects the catalytic modification effect on magnesium hydride.
[0108] 0.1 g gC3 N 4 / TiO 2 It was ball-milled with 0.9g of commercial magnesium hydride at a speed of 400r / min and a ball-milling time of 2h. The obtained composite sample was tested for hydrogen desorption and hydrogen absorption. The hydrogen desorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 500℃ at a heating rate of 5℃ / min. The amount of hydrogen released during this process was measured and drawn into a variable temperature hydrogen desorption curve. The hydrogen absorption performance test was as follows: 200mg of the composite sample was transferred to a hydrogen storage tester, and the temperature was increased from room temperature to 250℃ at a heating rate of 5℃ / min. A hydrogen pressure of 5MPa was provided at 250℃ and kept warm for 1.5h. The amount of hydrogen absorbed during this process was measured and drawn into an isothermal hydrogen absorption curve. Pure magnesium hydride was also tested for hydrogen desorption and hydrogen absorption performance under the same conditions, and the obtained performance was compared with gC 3 N 4 / TiO 2 The modified samples were compared.
[0109] After testing, gC 3 N 4 / TiO 2 Catalytically modified magnesium hydride can reduce the dehydrogenation temperature and increase the dehydrogenation and absorption capacity, but due to the serious agglomeration of titanium oxide particles, the catalytic modification effect is reduced (Comparative Example 1). The initial dehydrogenation temperature and peak dehydrogenation temperature of unmodified magnesium hydride are 317°C and 375°C, and the dehydrogenation rate is 93.1%. 3 N 4 / TiO 2 After modification, the initial dehydrogenation temperature and peak dehydrogenation temperature were reduced to 225℃ and 331℃, respectively, and the dehydrogenation rate was 93.3%. After 1.5h of hydrogen absorption, the hydrogen absorption of unmodified magnesium hydride was only 4.12wt.%, reaching only 54.2% of the hydrogen absorption rate, while gC 3 N 4 / TiO 2 The hydrogen absorption capacity of the catalytically modified magnesium hydride is 5.97wt.%, reaching a hydrogen absorption rate of 87.3%.
Claims
1. A hierarchical pore structure g-C3N4 / TiO2, characterized in that: The g-C3N4 / TiO2 is a g-C3N4 with a hierarchical pore structure, and the surface or pores of the g-C3N4 are uniformly loaded with TiO2 nanoparticles.
2. The hierarchical pore structure g-C3N4 / TiO2 according to claim 1, characterized in that: The pore size of g-C3N4 / TiO2 is 50-100nm, and the particle size of TiO2 nanoparticles is 100-200nm.
3. The method for preparing the hierarchical pore structure g-C3N4 / TiO2 according to claim 1 or 2, comprising the steps of: (1) Monodisperse SiO2 spheres and amino compounds are fully mixed and calcined to obtain g-C3N4 / SiO2; then SiO2 is removed by etching to obtain hierarchical pore structure g-C3N4; (2) Titanium tetrachloride, deionized water, ethylene glycol, and hierarchical pore structure g-C3N4 are fully mixed and dispersed uniformly, subjected to hydrothermal reaction, filtered, washed, and dried to obtain hierarchical pore structure g-C3N4 / TiO2.
4. The method for preparing the hierarchical pore structure g-C3N4 / TiO2 according to claim 3, characterized in that: In step (1), the method for preparing monodisperse SiO2 spheres comprises the steps of: uniformly mixing anhydrous ethanol, deionized water and concentrated ammonia water, dropwise adding tetraethyl orthosilicate, reacting, centrifuging, washing and drying to obtain monodisperse SiO2 spheres; Preferably, the mass concentration of concentrated ammonia water is 25% to 28%; the volume ratio of anhydrous ethanol to deionized water is (6 to 10):1; the volume ratio of deionized water to concentrated ammonia water is (2 to 3):1; the volume ratio of tetraethyl orthosilicate to deionized water is (0.3 to 0.5):1; Preferably, the reaction temperature is 40-50°C and the reaction time is 1-2h.
5. The method for preparing the hierarchical pore structure g-C3N4 / TiO2 according to claim 3, characterized in that: In step (1), one or more of the following conditions are included: i. The amino compound is one or a combination of two or more of urea, biuret, dicyandiamide or melamine; ii. The mass ratio of monodisperse SiO2 spheres to amino compounds is (0.025-3):1, preferably (0.2-3):1; iii. The calcination temperature is 550-600°C, the calcination time is 2-4h, and the calcination atmosphere is an inert gas; preferably, the inert gas is nitrogen or argon.
6. The method for preparing the hierarchical pore structure g-C3N4 / TiO2 according to claim 3, characterized in that: In step (1), the etching method comprises the steps of: immersing g-C3N4 / SiO2 in a corrosive solution, undergoing an etching reaction, filtering, washing, and drying to obtain hierarchical pore structure g-C3N4; Preferably, the etching liquid is one of a hydrofluoric acid aqueous solution or an ammonium bifluoride aqueous solution, and the concentration of the etching liquid is (2-5) mol / L; Preferably, the mass ratio of the monodisperse SiO2 spheres to the volume ratio of the etching solution is 1: (4-200) g / mL; Preferably, the etching reaction temperature is room temperature, the etching reaction is carried out under stirring conditions, and the etching reaction time is 12-24 hours.
7. The method for preparing the hierarchical pore structure g-C3N4 / TiO2 according to claim 3, characterized in that: In step (2), the volume ratio of titanium tetrachloride, deionized water and ethylene glycol is 1:(0.8-1.5):(25-45); the mass ratio of titanium tetrachloride to hierarchical pore structure g-C3N4 is (0.9-3.3):
1.
8. The method for preparing the hierarchical pore structure g-C3N4 / TiO2 according to claim 3, characterized in that: In step (2), the hydrothermal reaction temperature is 150-180° C., and the hydrothermal reaction time is 4-8 h.
9. Application of the hierarchical pore structure g-C3N4 / TiO2 as claimed in claim 1 or 2 in hydrogen storage.
10. The use according to claim 9, characterized in that: The application method comprises the steps of: ball-milling and mixing the hierarchical pore structure g-C3N4 / TiO2 and magnesium hydride to obtain a composite material for hydrogen storage; Preferably, the mass ratio of the hierarchical pore structure g-C3N4 / TiO2 to magnesium hydride is 1:5-15; the ball milling speed is 200-600r / min, and the ball milling time is 1-3h.
Citation Information
Patent Citations
Preparation method of cobalt-doped honeycomb-shaped graphite-phase carbon nitride nanomaterial and product
CN106744744A
Ordered hierarchical porous graphite-phase carbon nitride photocatalytic material preparation method
CN109126852A
Photocatalytic foliage fertilization method
CN111527851A
g-C3N4-based TiO2 crystal grain accumulation three-dimensional through hole composite structure and preparation method thereof
CN113117720A
Preparation method of high-conductivity lithium iron phosphate positive plate
CN114628637A
Cited By
Composite hydrogen storage material and preparation method thereof
CN122276666A
Composite hydrogen storage material and preparation method thereof
CN122276666B