Nitrogen-doped carbon-coated fluorine-doped titanium magnesium phosphate material as well as preparation method and application thereof

The preparation method of nitrogen-doped carbon-coated fluorine-doped titanium magnesium phosphate material solves the problem of the influence of titanium pyrophosphate impurities in the titanium magnesium phosphate material, improves the electrochemical performance and cycle performance of lithium-ion batteries, and achieves high efficiency, Low-cost battery material applications.

CN118754082APending Publication Date: 2024-10-11YIBIN NANMU NANO TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410915713.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Titanium magnesium phosphate materials produce titanium pyrophosphate impurities during the production process, which affects its purity and battery application performance. The initial electronic conductivity is low and needs to be improved through doping or coating.

Method used

The preparation method of nitrogen-doped carbon-coated fluorine-doped titanium magnesium phosphate material is adopted, and the formation of impurity titanium pyrophosphate is avoided through sand grinding, spray granulation and staged calcination, and the electrochemical performance of the material is improved.

Benefits of technology

It effectively improves the rate performance and cycle performance of titanium magnesium phosphate materials, increases the ion conductivity and cycle capacity retention rate of lithium-ion batteries, reduces material costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754082A_ABST
    Figure CN118754082A_ABST
Patent Text Reader

Abstract

The invention relates to a nitrogen-doped carbon-coated fluorine-doped titanium magnesium phosphate material and a preparation method and application thereof.The preparation method comprises the steps that a magnesium source material, a titanium source material, deionized water and a fatty acid dispersing agent are subjected to sanding treatment to obtain a mixed solution, a phosphorus source material is added, ammonium fluoride is added after uniform stirring, uniform mixing is conducted, spray granulation is conducted, and first solid particles are obtained; crushing the particles, calcining in a muffle furnace to obtain fluorine-doped magnesium titanium phosphate, ball-milling and crushing the fluorine-doped magnesium titanium phosphate, adding deionized water, continuously ball-milling until the particle size is less than or equal to 1 mu m, adding cane sugar and carbamide, uniformly mixing, performing spray granulation to obtain second solid particles, and ball-milling the second solid particles to obtain the fluorine-doped magnesium titanium phosphate. The particle size of the precursor material is smaller than or equal to 1 [mu] m, and then the precursor material is calcined twice to obtain the nitrogen-doped carbon-coated fluorine-doped titanium magnesium phosphate material. When the nitrogen-doped carbon-coated fluorine-doped titanium magnesium phosphate material is applied to the lithium ion battery, the cycle performance of the lithium ion battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy materials, and in particular to a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material and a preparation method and application thereof. Background Art

[0002] Solid-state battery technology is widely regarded as the next generation of battery technology with great potential. Compared with traditional liquid lithium batteries, solid-state batteries show significant advantages in energy density and safety, and have higher mechanical strength and stability. Solid electrolyte is one of the most important materials in solid-state batteries. Good conductivity and safety and reliability are the advantages of solid electrolyte materials.

[0003] With the great success of lithium-ion batteries, magnesium, which is located diagonally with lithium on the periodic table, has similar chemical properties to lithium and a small difference in ion radius. Its ions carry two charges, making it an ideal alternative material. Therefore, the use of magnesium in batteries has received increasing attention. As one of the most abundant light metal elements on earth, magnesium has good physical, chemical, and mechanical properties. Magnesium is an active metal with good thermal and electrical conductivity, but at the same time, magnesium is not as active as lithium. Therefore, it is easy to operate, safe, and inexpensive. Its price is only 1 / 24 of that of Li, it is pollution-free, and the magnesium negative electrode does not produce dendrites. Its theoretical volume energy density is 3833mA·h / cm 3 , much higher than the theoretical volume energy density of Li 2046mA·h / cm 3 . my country currently ranks first in the world in magnesium reserves and has a unique advantage in developing magnesium materials for batteries. The development of low-cost magnesium-containing materials that can improve the performance of existing batteries is considered an important direction for the development of secondary energy storage technology. Carrying out battery-related research work containing titanium magnesium phosphate materials is of great significance to the sustainable development of future energy.

[0004] Magnesium Titanium Phosphate (Mg 0.5 T i 2 (PO 4 ) 3 ) is a new type of solid electrolyte material with good electrochemical properties. However, in the prior art, the production process of magnesium titanium phosphate will produce titanium pyrophosphate impurity peaks, which will affect its purity and further affect its application performance in batteries. In addition, the initial magnesium titanium phosphate material has a low electronic conductivity, so it is often necessary to improve its conductivity by doping or coating. Summary of the invention

[0005] The embodiment of the present invention provides a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material and a preparation method and application thereof, the purpose of which is to solve the problem of magnesium titanium phosphate Mg 0.5 T i 2 (PO 4 )3 Titanium pyrophosphate impurity peaks will be generated during the production process, which will affect its purity and further affect its application performance in batteries. The electrochemical properties of the material are improved by doping fluorine and doping nitrogen in the carbon coating layer.

[0006] To this end, in a first aspect, an embodiment of the present invention provides a method for preparing a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, the preparation method comprising:

[0007] Step S1, weighing magnesium source material and titanium source material according to the stoichiometric ratio, placing them in a sand mill together with deionized water and a fatty acid dispersant, and performing sand milling to obtain a mixed solution; wherein the particle size D of the solid material in the mixed solution is V 50 is 1 μm;

[0008] Step S2, adding the phosphorus source material to the mixed solution and stirring it, adding ammonium fluoride after stirring it evenly, continuing to stir and mix it evenly, and then placing it in a vacuum spray dryer for the first spray granulation to obtain first solid particles;

[0009] Step S3, placing the first solid particles in a ball mill for ball milling, and then placing them in a muffle furnace for a first calcination treatment to obtain fluorine-doped magnesium titanium phosphate;

[0010] Step S4, placing fluorine-doped magnesium titanium phosphate in a ball mill, adding deionized water to continue ball milling until the particle size is less than or equal to 1 μm, adding sucrose and carbonamide, stirring and mixing evenly, placing in a vacuum spray dryer for a second spray granulation to obtain second solid particles;

[0011] Step S5, placing the second solid particles in a ball mill, and ball milling the particles to obtain a particle size D V Precursor materials with a diameter of 50 to less than or equal to 1 μm;

[0012] Step S6, placing the precursor material in a tube furnace for a second calcination treatment, and then performing a third calcination treatment to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0013] Preferably, the magnesium source material includes: magnesium oxide and / or magnesium hydroxide;

[0014] The titanium source material is titanium dioxide; the fatty acid dispersant includes one or more of palmitic acid, linolenic acid, stearic acid, lauric acid, acrylic acid, oleic acid or linoleic acid; the mass of the fatty acid dispersant accounts for 1%-5% of the total mass of the magnesium source material and the titanium source material;

[0015] The solid content of the mixed solution is 10wt%-20wt%.

[0016] Preferably, the phosphorus source material includes: one or more of diammonium phosphate, diammonium hydrogen phosphate, and concentrated phosphoric acid;

[0017] The mass percentage of the ammonium fluoride to the mixed solution is 0.1%-0.5%.

[0018] Preferably, the rotation speed of the sanding treatment in step S1 is 2300rpm-2700rpm, and the sanding time is 1.5 hours-2 hours;

[0019] The stirring speed in step S2 is 1000 rpm-1500 rpm, and the stirring time is 0.5 hour-1 hour.

[0020] Preferably, the specific conditions of the first spray granulation in step S2 and the second spray granulation in step S4 are: setting the inlet temperature of the spray dryer to 300° C., the outlet temperature to 170° C., and the pressure to 100 Pa-130 Pa.

[0021] Preferably, the temperature of the first calcination treatment in step S3 is between 800° C. and 1200° C., and the first calcination time is between 2 hours and 10 hours;

[0022] In the step S6, the temperature of the second calcination treatment is 400°C-500°C, and the second calcination treatment time is 1 hour-5 hours; the temperature of the third calcination treatment is 800-1200°C, and the third calcination treatment time is 2 hours-10 hours.

[0023] Preferably, the mass ratio of sucrose, carbonamide and fluorine-doped magnesium titanium phosphate in step S4 is 1: [0.1-0.5]: 2;

[0024] The rotation speed of the ball mill in step S5 is 100 rpm-150 rpm.

[0025] In a second aspect, an embodiment of the present invention provides a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material prepared by the preparation method described in the first aspect above.

[0026] In a third aspect, an embodiment of the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material according to the second aspect.

[0027] Preferably, the lithium-ion battery comprises an all-solid-state lithium-ion battery or a semi-solid-state lithium-ion battery.

[0028] The embodiment of the present invention provides a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material and a preparation method and application. The present invention sand-grinds a magnesium source material and a titanium source material with deionized water and a fatty acid dispersant to obtain a mixed solution, adds a phosphorus source material, stirs evenly, then adds ammonium fluoride, mixes evenly, and sprays granulates to obtain solid particles, ball-mills the material, and places the material in a muffle furnace for calcination to obtain fluorine-doped magnesium titanium phosphate, then ball-mills the fluorine-doped magnesium titanium phosphate, adds deionized water, and continues to ball-mill until the particle size is less than or equal to 1 μm, adds sucrose and carbonamide, mixes evenly, and then sprays granulates the material to obtain a second solid particle, and then ball-mills the second solid particle to obtain a particle size D V The precursor material is calcined in stages, first at low temperature and then at high temperature, to finally prepare a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0029] The preparation method of the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material provided in the embodiment of the present invention is to first mix the magnesium source and the titanium source evenly, and then add the phosphorus source to mix, so that the materials are mixed more evenly, wherein the powder particle size of the magnesium source and the titanium source is larger than that of the phosphorus source, and the hardness is harder, and it is not easy to grind down. In addition, due to the large difference in the ratio of magnesium to titanium and phosphorus, the magnesium content is relatively small, and it is not easy to mix evenly, and it is easy to produce impurity titanium pyrophosphate. The present invention makes the magnesium distribution more uniform through step-by-step mixing, thereby avoiding the formation of impurity non-conductive secondary phase titanium pyrophosphate, and obtaining a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material with higher purity, avoiding the influence of titanium pyrophosphate on material performance. The preparation method provided in the embodiment of the present invention is simple to operate, low in cost, and can be applied to large-scale production.

[0030] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material obtained by the above preparation method can effectively improve the rate performance of the magnesium titanium phosphate material by fluorine doping, and appropriate anion doping can suppress the dislocation defects of the material, which is beneficial to improve the Li + The diffusion kinetics of Li + The transmission channel mainly improves the rate cycling performance of the material. On the other hand, the nitrogen-doped carbon-coated material has a more superior electrochemical performance due to the introduction of nitrogen elements and the carbon-nitrogen covalent bond in the carbon coating layer. It is applied to lithium-ion batteries. The nitrogen atoms and fluorine atoms doped in the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material can improve the ionic conductivity of the material, thereby improving the cycling performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a flow chart of the preparation method of the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material provided by an embodiment of the present invention.

[0032] Figure 2This is a scanning electron microscope (SEM) image of the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material provided in Example 1 of the present invention.

[0033] Figure 3 : is the X-ray diffraction (XRD) pattern of the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material prepared in this embodiment. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments.

[0036] The present invention provides a method for preparing a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material. Figure 1 As shown, the following steps are included:

[0037] Step S1, weighing magnesium source material and titanium source material according to the stoichiometric ratio, placing them in a sand mill together with deionized water and a fatty acid dispersant, and performing sand milling to obtain a mixed solution; wherein the particle size D of the solid material in the mixed solution is V 50 is 1 μm;

[0038] Wherein, the magnesium source material includes: magnesium oxide and / or magnesium hydroxide;

[0039] The titanium source material is titanium dioxide;

[0040] The fatty acid dispersant includes: one or more of palmitoleic acid, linolenic acid, stearic acid, lauric acid, acrylic acid, oleic acid or linoleic acid; the mass of the fatty acid dispersant accounts for 1%-5% of the mass of the mixed solution;

[0041] The solid content in the mixed solution is 10wt%-20wt%;

[0042] The speed of sanding treatment is 2300rpm-2700rpm, and the sanding time is 1.5 hours-2 hours

[0043] The particle size D of the solid material in the mixed solution in this step V 50 is 1 μm, the purpose is to facilitate the subsequent spray granulation and avoid clogging the spray drying equipment. Smaller particle size can increase the reactivity of the material and make the particles obtained by spray granulation more uniform.

[0044] Step S2, adding the phosphorus source material to the mixed solution and stirring it, adding ammonium fluoride after stirring it evenly, continuing to stir and mix it evenly, and then placing it in a vacuum spray dryer for the first spray granulation to obtain first solid particles;

[0045] Wherein, the phosphorus source material is weighed according to the stoichiometric ratio of titanium magnesium phosphate, including one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and concentrated phosphoric acid;

[0046] The mass percentage of ammonium fluoride in the mixed solution is 0.1%-0.5%;

[0047] The stirring speed is 1000rpm-1500rpm, and the stirring time is 0.5 hour-1 hour;

[0048] The specific conditions of the first spray granulation in this step are: the inlet temperature of the spray dryer is set to 300°C, the outlet temperature is set to 170°C, and the pressure is set to 100Pa-130Pa. Step S3, the first solid particles are placed in a ball mill for ball milling, and then placed in a muffle furnace for a first calcination treatment to obtain fluorine-doped magnesium titanium phosphate;

[0049] The temperature of the first calcination treatment is between 800°C and 1200°C, and the first calcination time is between 2 hours and 10 hours;

[0050] The chemical formula of fluorine-doped magnesium titanium phosphate is Mg 0.5 T i 2 (PO 3 ) 3 O 3-x F 2x , where 0<x<0.1;

[0051] Fluorine doping to replace oxygen atoms can effectively improve the rate performance of magnesium titanium phosphate materials. This is because fluorine doping as an anion can inhibit the dislocation defects of the material, which is beneficial to improving the diffusion dynamics of lithium ions and will not block the lithium ion transmission channel, thereby improving the rate cycling performance of the material.

[0052] Step S4, placing fluorine-doped magnesium titanium phosphate in a ball mill, adding deionized water to continue ball milling until the particle size is less than or equal to 1 μm, adding sucrose and carbonamide, stirring and mixing evenly, placing in a vacuum spray dryer for a second spray granulation to obtain second solid particles;

[0053] The mass ratio of sucrose, carbonamide and fluorine-doped magnesium titanium phosphate is 1: [0.1-0.5]: 2;

[0054] The specific conditions of the second spray granulation are: setting the inlet temperature of the spray dryer to 300°C, the outlet temperature to 170°C, and the pressure to 100Pa-130Pa.

[0055] Step S5, placing the second solid particles in a ball mill, and ball milling the particles to obtain a particle size D V Precursor materials with a diameter of 50 to less than or equal to 1 μm;

[0056] Among them, the rotation speed of the ball mill is 100rpm-150rpm.

[0057] Step S6, placing the precursor material in a tube furnace for a second calcination treatment, and then performing a third calcination treatment to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0058] The temperature of the second calcination treatment is 400°C-500°C, and the second calcination treatment time is 1 hour-5 hours; the temperature of the third calcination treatment is 800-1200°C, and the third calcination treatment time is 2 hours-10 hours.

[0059] The method for preparing the above-mentioned nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material provided by an embodiment of the present invention is to first mix the magnesium source and the titanium source evenly, and then add the phosphorus source to mix, so that the material mixing is more even, wherein the powder particle size of the magnesium source and the titanium source is larger than that of the phosphorus source, and the hardness is harder, and it is not easy to grind down. In addition, due to the large difference in the ratio of magnesium, titanium and phosphorus, the magnesium content is relatively small, it is not easy to mix evenly, and it is easy to produce impurity titanium pyrophosphate. The present invention makes the magnesium distribution more uniform through step-by-step mixing, thereby avoiding the generation of impurity pyrophosphate, and obtaining a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material with higher purity, thereby avoiding the influence of titanium pyrophosphate on material properties.

[0060] In the embodiment of the present invention, the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material obtained by the above preparation method can effectively improve the rate performance of the magnesium titanium phosphate material by fluorine doping, and appropriate anion doping can suppress the dislocation defects of the material, which is beneficial to improve the Li + The diffusion kinetics of Li + The transmission channel mainly improves the rate cycling performance of the material; on the other hand, the nitrogen-doped carbon-coated material has a more superior electrochemical performance due to the introduction of nitrogen elements and the presence of carbon-nitrogen covalent bonds in the carbon coating layer. The morphology and conductivity of the doped material can be effectively controlled by adjusting the nitrogen doping amount, thereby improving the cycling performance of the material.

[0061] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material prepared by the above preparation method provided in the embodiment of the present invention can be used as a solid electrolyte membrane in a lithium-ion battery, which includes an all-solid-state lithium-ion battery or a semi-solid-state lithium-ion battery. Among them, the method of using nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material to prepare a solid electrolyte membrane is an existing known conventional method, including but not limited to a solid phase reaction method, a sol-gel method, an electrochemical deposition method or a water-based flow edge method. And the positive and negative electrodes of the lithium-ion battery are both prepared by existing known methods, and the positive electrode active material and the negative electrode active material are both commonly used materials.

[0062] In order to better understand the technical solution provided by the present invention, the preparation method and characteristics of the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of the present invention are respectively described below with specific examples.

[0063] Example 1

[0064] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0065] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 26 g of palmitic acid in a sand mill, and perform sand milling at a speed of 2700 rpm for 1.5 hours to obtain a solid material particle size D V 50

[0066] A mixed solution of 1 μm.

[0067] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 5 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0068] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1000° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0069] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm. 200 g of sucrose and 20 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0070] (5) The second solid particles are placed in a ball mill and subjected to ball milling at a speed of 150 rpm to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0071] (6) The precursor material is placed in a tube furnace and calcined at 500° C. for 1 hour, and then the temperature is raised to 1000° C. and calcined for 2 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0072] The SEM image of the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material prepared in this embodiment is as follows: Figure 2 shown.

[0073] The XRD pattern of the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material prepared in this embodiment is as follows: Figure 3 shown.

[0074] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment is used to prepare a solid electrolyte membrane and assemble it into an all-solid-state lithium-ion battery for performance testing. The specific process is as follows:

[0075] Preparation of solid electrolyte membrane: This embodiment adopts the conventional method water-based flow-edge method to prepare solid electrolyte membrane using nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material (the preparation process also adds water-soluble dispersant sodium polyacrylate, water-soluble binder sodium carboxymethyl cellulose and water-soluble auxiliary agent octylphenol polyoxyethylene ether).

[0076] Preparation of positive electrode sheet: The positive electrode active material lithium iron phosphate (LiFePO 4 ), conductive agent (Super P), binder (PVDF) are mixed in a mass ratio of 85:10:5, and then solvent (NMP) is added. After stirring for 12 hours, a viscous slurry is formed and evenly coated on the surface of the current collector aluminum foil. Dry in a 60°C blast drying oven for 12 hours, then transfer to a 100°C vacuum drying oven for 1 hour, and punch out into positive electrode sheets with a diameter of 12 mm.

[0077] Assembling all-solid-state lithium-ion batteries: assemble in the order of negative electrode shell, lithium sheet, solid electrolyte membrane, positive electrode sheet, gasket, shrapnel, and positive electrode shell, and do not use any electrolyte during the assembly process. The assembly is an all-solid-state lithium-ion battery, and the assembly process is completed in a glove box containing a high-purity Ar atmosphere.

[0078] Testing of all-solid-state lithium batteries:

[0079] The ionic conductivity of the assembled all-solid-state lithium battery was tested on an electrochemical workstation using a conventional method.

[0080] The above-assembled all-solid-state lithium battery was subjected to charge and discharge test on a charge and discharge tester, with the test voltage range of 2.7V-4V. The battery was subjected to charge and discharge cycle test at a rate of 0.1C, and the cycle capacity retention rate was tested for 500 cycles.

[0081] The test data of ionic conductivity and cycle capacity retention rate are shown in Table 1.

[0082] Example 2

[0083] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0084] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 26 g of linolenic acid in a sand mill, and perform sand milling at a speed of 2300 rpm for 2 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0085] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 6 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0086] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 800° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0087] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm. 200 g of sucrose and 20 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0088] (5) The second solid particles are placed in a ball mill and subjected to ball milling treatment at a rotation speed of 100 rpm to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0089] (6) The precursor material is placed in a tube furnace and calcined at 500° C. for 1 hour, and then the temperature is raised to 1000° C. and calcined for 2 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0090] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0091] Example 3

[0092] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0093] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them in a sand mill together with 4500 ml of deionized water and 26 g of stearic acid, and perform sand milling at a speed of 2300 rpm for 1.5 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0094] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 1 hour. After stirring evenly, 7 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0095] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1000° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0096] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm. 200 g of sucrose and 20 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0097] (5) Place the second solid particles in a ball mill and perform ball milling to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0098] (6) The precursor material is placed in a tube furnace and calcined at 500° C. for 1 hour, and then the temperature is raised to 1000° C. and calcined for 2 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0099] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0100] Example 4

[0101] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0102] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 26 g of palmitic acid in a sand mill, and perform sand milling at a speed of 2300 rpm for 1.5 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0103] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 8 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0104] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1000° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0105] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm, 200 g of sucrose and 25 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0106] (5) Place the second solid particles in a ball mill and perform ball milling to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0107] (6) The precursor material is placed in a tube furnace and calcined at 500° C. for 1 hour, and then the temperature is raised to 1000° C. and calcined for 2 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0108] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0109] Example 5

[0110] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0111] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 26 g of palmitic acid in a sand mill, and perform sand milling at a speed of 2300 rpm for 1.5 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0112] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 5 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0113] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1000° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0114] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added and the ball milling was continued until the particle size was less than or equal to 1 μm. 200 g of sucrose and 28 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0115] (5) Place the second solid particles in a ball mill and perform ball milling to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0116] (6) The precursor material is placed in a tube furnace and calcined at 500° C. for 1 hour, and then the temperature is raised to 1000° C. and calcined for 2 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0117] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0118] Example 6

[0119] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0120] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 26 g of palmitic acid in a sand mill, and perform sand milling at a speed of 2300 rpm for 1.5 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0121] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 5 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0122] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1000° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0123] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm. 200 g of sucrose and 30 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0124] (5) Place the second solid particles in a ball mill and perform ball milling to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0125] (6) The precursor material is placed in a tube furnace and calcined at 500° C. for 1 hour, and then the temperature is raised to 1000° C. and calcined for 2 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0126] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0127] Example 7

[0128] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0129] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 26 g of palmitic acid in a sand mill, and perform sand milling at a speed of 2300 rpm for 1.5 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0130] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 10 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0131] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1000° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0132] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm, 200 g of sucrose and 25 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0133] (5) Place the second solid particles in a ball mill and perform ball milling to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0134] (6) The precursor material is placed in a tube furnace and calcined at 500° C. for 1 hour, and then the temperature is raised to 1000° C. and calcined for 2 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0135] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0136] Example 8

[0137] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0138] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 26 g of palmitic acid in a sand mill, and perform sand milling at a speed of 2300 rpm for 1.5 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0139] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 5 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0140] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1200° C. for 3 hours to obtain fluorine-doped magnesium titanium phosphate.

[0141] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm. 200 g of sucrose and 20 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0142] (5) Place the second solid particles in a ball mill and perform ball milling to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0143] (6) The precursor material is placed in a tube furnace and calcined at 400° C. for 5 hours, and then the temperature is raised to 1200° C. and calcined for 3 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0144] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0145] Example 9

[0146] This embodiment provides a preparation process and performance test of a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, and the specific process is as follows:

[0147] (1) Weigh 20 g of magnesium oxide and 160 g of titanium dioxide, place them together with 2000 ml of deionized water and 30 g of acrylic acid in a sand mill, and perform sand milling at a speed of 2300 rpm for 1.5 hours to obtain a solid material particle size D V 50 is a mixed solution of 1 μm.

[0148] (2) 345 g of ammonium dihydrogen phosphate was added to the mixed solution for stirring at a speed of 1000 rpm for 0.5 hour. After stirring evenly, 8 g of ammonium fluoride was added and the mixture was stirred and mixed evenly. The mixture was then placed in a vacuum spray dryer for the first spray granulation to obtain first solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0149] (3) The first solid particles were placed in a ball mill for ball milling, and then placed in a muffle furnace for calcination at 1000° C. for 5 hours to obtain fluorine-doped magnesium titanium phosphate.

[0150] (4) 400 g of fluorine-doped magnesium titanium phosphate was placed in a ball mill, and after ball milling, deionized water was added to continue ball milling until the particle size was less than or equal to 1 μm, 200 g of sucrose and 25 g of carbonamide were added and stirred to mix evenly, and then placed in a vacuum spray dryer for a second spray granulation to obtain second solid particles, wherein the inlet temperature of the spray dryer was 300° C., the outlet temperature was 170° C., and the pressure was 100 Pa.

[0151] (5) Place the second solid particles in a ball mill and perform ball milling to obtain a particle size D V 50 to less than or equal to 1μm precursor material.

[0152] (6) The precursor material is placed in a tube furnace and calcined at 400° C. for 5 hours, and then the temperature is raised to 1200° C. and calcined for 3 hours to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

[0153] The nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of this embodiment was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.

[0154] In order to better illustrate the effects of the embodiments of the present invention, comparative examples 1-3 are compared with the above embodiments.

[0155] Comparative Example 1

[0156] This comparative example provides a preparation process and performance test of carbon-coated magnesium titanium phosphate. The difference from Example 1 is that this comparative example is not doped with fluorine and nitrogen, that is, ammonium fluoride is not added in step (2), and carbonamide is not added in step (4). The other preparation processes are the same as those in Example 1.

[0157] The carbon-coated magnesium titanium phosphate of this comparative example was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as that of Example 1. The test data is detailed in Table 1.

[0158] Comparative Example 2

[0159] This comparative example provides a preparation process and performance test of nitrogen-doped carbon-coated magnesium titanium phosphate. The difference from Example 1 is that this comparative example is not doped with fluorine, that is, ammonium fluoride is not added in step (2). The other preparation processes are the same as those in Example 1.

[0160] The nitrogen-doped carbon-coated magnesium titanium phosphate of this comparative example was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as that of Example 1. The test data is detailed in Table 1.

[0161] Comparative Example 3

[0162] This comparative example provides a preparation process and performance test of carbon-coated fluorine-doped magnesium titanium phosphate. The difference from Example 1 is that this comparative example is not doped with nitrogen, that is, no carbonamide is added in step (4). The other preparation processes are the same as those in Example 1.

[0163] The carbon-coated fluorine-doped magnesium titanium phosphate of this comparative example was used to prepare a solid electrolyte membrane and assembled into an all-solid-state lithium-ion battery for performance testing. The specific process was the same as that of Example 1. The test data is detailed in Table 1.

[0164] Table 1 is a summary of the test data of the all-solid-state lithium-ion batteries assembled in Examples 1-9 and Comparative Examples 1-2:

[0165] Serial number <![CDATA[Ionic conductivity (S.cm -1 )]]> Cycle capacity retention rate (%) Example 1 <![CDATA[5.1×10 -4 ]]> 96 Example 2 <![CDATA[7.6×10 -4 ]]> 95 Example 3 <![CDATA[7.2×10 -4 ]]> 96 Example 4 <![CDATA[6.9×10 -4 ]]> 97 Example 5 <![CDATA[6.6×10 -4 ]]> 98 Example 6 <![CDATA[7.0×10 -4 ]]> 97 Example 7 <![CDATA[5.4×10 -4 ]]> 95 Example 8 <![CDATA[5.3×10 -4 ]]> 97 Example 9 <![CDATA[5.8×10 -4 ]]> 97 Comparative Example 1 <![CDATA[9.0×10 -5 ]]> 81 Comparative Example 2 <![CDATA[8.6×10 -5 ]]> 86 Comparative Example 3 <![CDATA[9.9×10 -5 ]]> 82

[0166] Table 1

[0167] By comparing the test data in Table 1, it can be seen that the ionic conductivity and cycle capacity retention rate of Examples 1-9 are better than those of the batteries assembled in Comparative Examples 1-3. This is because the solid electrolyte membrane prepared by the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material of the present invention is used in the all-solid-state lithium-ion batteries assembled in Examples 1-9. The fluorine ions doped in the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material can suppress the dislocation defects of the material, which is beneficial to improve the Li + The diffusion kinetics of Li +The transmission channel can effectively improve the rate performance of the magnesium titanium phosphate material. In addition, the nitrogen ions doped in the carbon coating layer have a covalent bond with the carbon, which makes it have more superior electrochemical performance. The doped nitrogen atoms and fluorine atoms can improve the ionic conductivity of the material, thereby improving the cycle performance of the lithium ion battery. In addition, in the process of preparing the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, the preparation process adopted by the present invention inhibits the formation of the non-conductive secondary phase titanium pyrophosphate, effectively reducing the hindering effect in the ion migration process, thereby further improving the ionic conductivity.

[0168] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material, characterized in that: The preparation method comprises: Step S1, weighing magnesium source material and titanium source material according to the stoichiometric ratio, placing them in a sand mill together with deionized water and a fatty acid dispersant, and performing sand milling to obtain a mixed solution; wherein the particle size D of the solid material in the mixed solution is V 50 is 1 μm; Step S2, adding the phosphorus source material to the mixed solution and stirring it, adding ammonium fluoride after stirring it evenly, continuing to stir and mix it evenly, and then placing it in a vacuum spray dryer for the first spray granulation to obtain first solid particles; Step S3, placing the first solid particles in a ball mill for ball milling, and then placing them in a muffle furnace for a first calcination treatment to obtain fluorine-doped magnesium titanium phosphate; Step S4, placing fluorine-doped magnesium titanium phosphate in a ball mill, adding deionized water to continue ball milling until the particle size is less than or equal to 1 μm, adding sucrose and carbonamide, stirring and mixing evenly, placing in a vacuum spray dryer for a second spray granulation to obtain second solid particles; Step S5, placing the second solid particles in a ball mill, and ball milling the particles to obtain a particle size D V Precursor materials with a diameter of 50 to less than or equal to 1 μm; Step S6, placing the precursor material in a tube furnace for a second calcination treatment, and then performing a third calcination treatment to obtain a nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material.

2. The preparation method according to claim 1, characterized in that: The magnesium source material includes: magnesium oxide and / or magnesium hydroxide; the titanium source material is titanium dioxide; The fatty acid dispersant includes: one or more of palmitoleic acid, linolenic acid, stearic acid, lauric acid, acrylic acid, oleic acid or linoleic acid; the mass of the fatty acid dispersant accounts for 1%-5% of the total mass of the magnesium source material and the titanium source material; The solid content of the mixed solution is 10wt%-20wt%.

3. The preparation method according to claim 1, characterized in that: The phosphorus source material includes: one or more of diammonium phosphate, diammonium hydrogen phosphate, and concentrated phosphoric acid; The mass percentage of the ammonium fluoride to the mixed solution is 0.1%-0.5%.

4. The preparation method according to claim 1, characterized in that: The rotation speed of the sanding treatment in step S1 is 2300 rpm-2700 rpm, and the sanding time is 1.5 hours-2 hours; The stirring speed in step S2 is 1000 rpm-1500 rpm, and the stirring time is 0.5 hour-1 hour.

5. The preparation method according to claim 1, characterized in that: The specific conditions of the first spray granulation in step S2 and the second spray granulation in step S4 are: setting the inlet temperature of the spray dryer to 300° C., the outlet temperature to 170° C., and the pressure to 100 Pa-130 Pa.

6. The preparation method according to claim 1, characterized in that: The temperature of the first calcination treatment in step S3 is between 800° C. and 1200° C., and the first calcination time is between 2 hours and 10 hours; In the step S6, the temperature of the second calcination treatment is 400°C-500°C, and the second calcination treatment time is 1 hour-5 hours; the temperature of the third calcination treatment is 800-1200°C, and the third calcination treatment time is 2 hours-10 hours.

7. The preparation method according to claim 1, characterized in that: The mass ratio of sucrose, carbonamide and fluorine-doped magnesium titanium phosphate in step S4 is 1: [0.1-0.5]: 2; The rotation speed of the ball mill in step S5 is 100 rpm-150 rpm.

8. A nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material prepared by the preparation method according to any one of claims 1 to 7.

9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the nitrogen-doped carbon-coated fluorine-doped magnesium titanium phosphate material according to claim 8.

10. The lithium ion battery according to claim 9, characterized in that: The lithium ion battery includes an all-solid lithium ion battery or a semi-solid lithium ion battery.

Citation Information

Patent Citations

  • Titanium and zirconium co-doped carbon-coated lithium iron phosphate material as well as preparation method and application thereof

    CN114314548A

  • Carbon-coated titanium magnesium phosphate electrode material, preparation method thereof and carbon-coated titanium magnesium phosphate composite electrode

    CN115548304A

  • Magnesium-based solid electrolyte, preparation method therefor, and battery

    WO2024021822A1