Preparation method and application of composite phosphoric acid material precursor
Controlling the distribution of Mn elements through the preparation method solves the problem of manganese element dissolution in lithium batteries from LMFP materials, improves cycle stability and battery performance, simplifies the process flow, and promotes its industrialization process.
Patent Information
- Application Number
- CN202410939985.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-11
AI Technical Summary
The problem of manganese dissolution of lithium iron manganese phosphate (LMFP) materials during the charging and discharging process of lithium batteries leads to a decrease in battery capacity and deterioration in cycle performance, which affects safety. In addition, the existing modification methods are technically difficult and costly to process, which limits their use. industrialization process.
A method for preparing the precursor of a composite phosphoric acid material is adopted. By configuring a bottom liquid, a metal solution and a phosphate solution in an inert gas atmosphere, and controlling the pH value and calcination temperature, a composite phosphoric acid material is obtained in which the Mn element content gradually decreases from the core to the outer shell. Precursor, reduce the dissolution of Mn element, improve cycle stability, and prepare the composite phosphoric acid material through the calcination reaction of the lithium source and the precursor of the composite phosphoric acid material.
It improves the cycle stability and battery performance of the composite phosphoric acid material, simplifies the preparation process, facilitates large-scale industrial application, and improves the safety and energy density of the battery.
Smart Images

Figure BDA0004944991340000071 
Figure BDA0004944991340000111 
Figure BDA0004944991340000121
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials, and in particular relates to a preparation method of a composite phosphoric acid material precursor and application thereof. Background Art
[0002] Lithium manganese iron phosphate (LiMnFePO4, LMFP for short) and lithium iron phosphate (LiFePO4, LFP for short) are both phosphate-based lithium-ion battery cathode materials. LMFP is a new type of material obtained by adding manganese to LFP. It retains the olivine structure of lithium iron phosphate, and at the same time improves the voltage platform and energy density of the material by adding manganese. LMFP has the advantages of low production cost, high energy density, green environmental protection, and good structural stability, and has broad application prospects in consumer electronics, new energy vehicles, and energy storage systems.
[0003] However, despite its many advantages, LMFP also faces some technical challenges. For example, the conductivity of LMFP is relatively low, and its performance needs to be improved through modification. Common modification methods include ion doping, surface coating, and micromorphology control. However, the above-mentioned modification methods will limit the industrialization process of LMFP due to the difficulty of processing technology and high cost of production line construction. In addition, the problem of manganese dissolution is a technical difficulty encountered by LMFP during the battery charging and discharging process, which will lead to a decrease in battery capacity, deterioration of cycle performance, and even affect the safety of the battery. The root of this problem lies in the special physical and chemical properties of manganese, especially its behavior during the charging and discharging process.
[0004] In the future, LMFP is rising in the lithium battery market, especially in the fields of new energy vehicles and energy storage systems. With the advancement of technology and the growth of market demand, LMFP's market share is expected to increase further. Therefore, companies and research institutions are currently working to solve existing technical challenges to achieve large-scale commercial production of LMFP. Summary of the invention
[0005] In order to improve the problem of manganese dissolution and at the same time provide a simple and convenient method for preparing phosphate-based electrode materials, the present invention provides a method for preparing a composite phosphoric acid material precursor and its application.
[0006] According to one aspect of the present invention, a method for preparing a composite phosphoric acid material precursor is provided, and the method comprises the following steps: S1. separately preparing a base liquid, a metal solution, and a phosphate solution, wherein the base liquid is an ammonia solution with a concentration of 1 to 8 g / L; the metal solution comprises at least one of a metal element and a water-soluble complexing agent, and the metal element comprises at least one of an Fe element and an Mn element; in the metal solution, the molar ratio of the Fe element: the Mn element: the water-soluble complexing agent is 0 to 10: 0 to 8: 0 to 5; S2. in an inert gas atmosphere, adding a metal solution, a phosphate solution, and a pH adjusting agent to the base liquid in parallel; S3. after adjusting the pH of the reaction system to 4 to 9, stopping the liquid addition, and performing an aging treatment; S4. performing solid-liquid separation on the reaction solution, and calcining the obtained solid under an inert gas atmosphere to obtain a composite phosphoric acid material precursor.
[0007] The preparation method provided by the present invention can obtain a composite phosphoric acid material precursor whose Mn content gradually decreases from the inner core to the outer shell, and the composite phosphoric acid material precursor can reduce the Mn content on its surface, thereby improving the problem of Mn element dissolution in the composite phosphoric acid material using the precursor and improving its cycle stability. In addition, the preparation method provided by the present invention is simple and convenient, which is conducive to large-scale industrial application.
[0008] Preferably, the metal solution is prepared from at least one of a water-soluble chelating agent, a water-soluble iron source, and a water-soluble manganese source; wherein the water-soluble iron source includes at least one of ferrous sulfate, ferric sulfate, ferric nitrate, and ferric chloride, and / or the water-soluble manganese source includes at least one of manganese sulfate, manganese nitrate, manganese chloride, and manganese acetate.
[0009] Preferably, the phosphate solution is prepared from water-soluble phosphates, wherein the water-soluble phosphates include at least one of phosphoric acid, ammonium monohydrogen phosphate, and ammonium dihydrogen phosphate.
[0010] Preferably, in the metal solution, the molar amount of the water-soluble complexing agent is 10-50% of the molar amount of the iron element, and the water-soluble complexing agent includes at least one of ethylenediaminetetraacetic acid (EDTA), potassium thiocyanate (KSCN), sodium citrate, and vitamin C.
[0011] Preferably, the metal solution includes at least one of metal solution A, metal solution B, metal solution C, metal solution D, metal solution E, and metal solution F; wherein, in metal solution A, calculated by molar ratio, Fe element: Mn element: water-soluble complexing agent = 0:1:0; in metal solution B, calculated by molar ratio, Fe element: Mn element: water-soluble complexing agent = 2:8:1; in metal solution C, calculated by molar ratio, Fe element: Mn element: water-soluble complexing agent = 4:6:2; in metal solution D, calculated by molar ratio, Fe element: Mn element: water-soluble complexing agent = 6:4:3; in metal solution E, calculated by molar ratio, Fe element: Mn element: water-soluble complexing agent = 8:2:4; in metal solution F, calculated by molar ratio, Fe element: Mn element: water-soluble complexing agent = 10:0:5. The ratio of Mn, Fe and chelating agent in the metal solution will affect the morphology of the amorphous phosphorus-deficient manganese iron phosphate precipitate formed in S2, and further affect the distribution of Mn and Fe elements in the composite phosphate material precursor.
[0012] Preferably, in S2, the metal solution includes metal solution A, metal solution F, and also includes at least one of metal solution B, metal solution C, metal solution D, and metal solution E; the added metal solutions are replaced in order of increasing molar content of the iron element at intervals of 20 to 120 minutes. By controlling the type of metal solution and the interval time of replacement, the content and thickness of manganese iron phosphate in the composite phosphoric acid material precursor can be controlled. In addition, the Mn element content can be controlled to not only gradually decrease from the inner core to the outer shell, but also to be distributed in a gradient concentration.
[0013] Preferably, the metal solution includes metal solution A, metal solution B, metal solution C, metal solution D, metal solution E, and metal solution F. Calculated by mass ratio, metal solution A: metal solution B: metal solution C: metal solution D: metal solution E: metal solution F = 0.5~1: 0.5~2: 0.5~2: 0.5~2: 0.5~2: 0.5~1.
[0014] Preferably, in S1, calculated by mass ratio, base solution: metal solution: phosphate solution = 0.5-1: 10-20: 10-20.
[0015] Preferably, in S1-S3, the reaction temperature is 20-90°C, and the stirring speed is 300-1000 rpm.
[0016] Preferably, in the metal solution, the water-soluble complexing agent is ethylenediaminetetraacetic acid, and the pH of the metal solution is 2-10, and the reaction temperature of the reaction system in S2 is 30-90°C.
[0017] Preferably, the water-soluble complexing agent is potassium thiocyanate, and the pH is 4-10, and the reaction temperature of the reaction system in S2 is 40-80°C.
[0018] Preferably, the water-soluble complexing agent is sodium citrate, and the pH is 3-10, and the reaction temperature of the reaction system in S2 is 50-90°C.
[0019] The pH in the metal solution (generally refers to the pH at room temperature, measured by the pH meter Mettler Toledo InPro4800i at 25°C) will affect the complexation reaction between iron ions and the complexing agent. Among them, the effect of pH on the complexation reaction is mainly reflected in its ability to change the charge state of the ligand and the central metal ion, thereby affecting the rate and equilibrium position of the complexation reaction. At different pH values, the morphology of metal ions and ligands may be different, which will affect their interactions and the stability of the complex. For example, under acidic conditions, some gold ions may exist in a multivalent form, while under alkaline conditions they may exist in a low-valent form, which will affect their ability to bind to the ligand.
[0020] The effect of reaction temperature on complex reaction is usually manifested as increasing temperature will accelerate the rate of complex reaction, but this is not absolute. Some reactions are more favorable at low temperatures, because high temperature may reduce the activity of reactants and affect the reaction effect. In addition, temperature will also affect the stability of the complex. Generally speaking, as the temperature increases, the complex equilibrium moves toward the metal ion direction (dissociation direction) because some complexes will dissociate at high temperatures. Therefore, the specific reaction temperature needs to be determined according to the phosphorus-deficient ferromanganese phosphate precipitation formed at each stage.
[0021] Preferably, the pH adjuster comprises aqueous ammonia.
[0022] Preferably, in S3, the aging treatment is: aging at 20 to 90° C. for 2 to 5 hours.
[0023] Preferably, the calcination treatment in S4 is carried out at a reaction temperature of 400 to 800° C. for 1 to 10 hours.
[0024] The second aspect of the present invention provides a composite phosphoric acid material, which is prepared by calcining a lithium source and a composite phosphoric acid material precursor, and the composite phosphoric acid material precursor is prepared by the above-mentioned preparation method. In the prior art of the present invention, the John-Teller effect of manganese ions causes the dissolution of manganese elements, which reduces the cycle life of the battery. The present invention, through structural design, can obtain a composite phosphoric acid material in which the Mn element content gradually decreases from the inner core to the outer shell and the Mn element is distributed in a gradient concentration, and the composite phosphoric acid material has good cycle performance.
[0025] Preferably, the calcination reaction is performed at 700-900°C.
[0026] Preferably, calculated by mass ratio, the composite phosphate material precursor: lithium source = 3-4: 1-1.5.
[0027] Preferably, the composite phosphoric acid material further comprises a carbon coating layer.
[0028] Preferably, the composite phosphoric acid material is prepared by calcining a lithium source, a carbon source and a composite phosphoric acid material precursor. Calculated by mass ratio, the composite phosphoric acid material precursor: lithium source: coated carbon source = 3-4: 1-1.5: 0.5-1.
[0029] Preferably, the carbon source comprises at least one of PEG, glucose, phenolic resin and starch.
[0030] The third aspect of the present invention provides an electrode, which includes the composite phosphoric acid material as described above.
[0031] A fourth aspect of the present invention provides a battery, comprising the electrode as described above. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0033] Example 1
[0034] (1) Raw materials required for preparing electrode materials
[0035] The raw materials required for preparing the electrode material in this embodiment are shown in Table 1, and the corresponding solutions are configured according to Table 1, wherein the water-soluble iron source is ferric sulfate, the water-soluble manganese source is manganese sulfate, the water-soluble chelating agent is EDTA; the water-soluble phosphate is ammonium dihydrogen phosphate; the pH regulator is ammonia water; the Fe element, the Mn element, and the water-soluble chelating agent in each metal solution are in a molar ratio.
[0036] Table 1. Raw materials required for preparing electrode materials in this example
[0037] Components Raw material composition Number of copies / pieces Primer Ammonia water, concentration 4g / L 1 Metal solution A Fe element: Mn element: water-soluble complexing agent = 0:1:0 1 Metal solution B Fe element: Mn element: water-soluble complexing agent = 2:8:1 2 Metal solution C Fe element: Mn element: water-soluble complexing agent = 4:6:2 2 Metal solution D Fe element: Mn element: water-soluble complexing agent = 6:4:3 2 Metal solution E Fe element: Mn element: water-soluble complexing agent = 8:2:4 2 Metal solution F Fe element: Mn element: water-soluble complexing agent = 10:0:5 1
[0038] (2) Preparation of composite phosphoric acid material precursor
[0039] S1. The base solution, metal solution A, metal solution B, metal solution C, metal solution D, metal solution E, metal solution F, and phosphate solution are configured according to Table 1;
[0040] S2. In an inert gas atmosphere, a metal solution, a phosphate solution and a pH adjuster are added to the base liquid in parallel, wherein the order of adding the metal solution is:
[0041] At 30°C, metal solution A (pH = 3) continued to flow for 30 minutes;
[0042] Then, metal solution A was replaced with metal solution B, and metal solution B (pH = 4.5) continued to flow for 20 minutes at 40°C;
[0043] Then, metal solution B was replaced with metal solution C, and metal solution B (pH=4.5) continued to flow for 40 minutes at 40°C;
[0044] Then, metal solution C was replaced with metal solution D, and metal solution B (pH = 4.5) continued to flow for 60 minutes at 40°C;
[0045] Then, metal solution D was replaced with metal solution E, and metal solution B (pH=6) continued to flow for 100 min at 50°C;
[0046] Then, metal solution E was replaced with metal solution F, and metal solution B (pH=6) continued to flow for 120 min at 50°C;
[0047] S3. The pH of the reaction system was adjusted to 7 by a pH adjusting agent, and then the liquid was stopped and the reaction was aged (reacted at a temperature of 50 ° C for 3 hours);
[0048] S4. The reaction solution is subjected to solid-liquid separation treatment, and the obtained solid is calcined under the protection of an inert gas (the reaction temperature is calcined at 600° C. for 5 hours) to obtain a composite phosphoric acid material precursor.
[0049] (3) Preparation of composite phosphoric acid materials
[0050] 810g of composite phosphate material precursor, 205.6g of lithium carbonate, 14g of PEG8000 and 84g of glucose were added with 1500g of deionized water and ground for 4h to obtain a slurry with a particle size of less than 0.5μm. The slurry was spray-dried. After drying, the sprayed material was placed in a nitrogen atmosphere furnace, heated to 700℃ at a heating rate of 5℃ / min, and calcined at a constant temperature for 12 hours, and then cooled to room temperature to obtain a sintered material. The sintered material was crushed to obtain an electrode material.
[0051] (4) Preparation of batteries
[0052] Lithium manganese iron phosphate positive electrode material, acetylene black as conductive agent, PVDF as binder, mixed at a mass ratio of 9:0.2:0.8, and added a certain amount of organic solvent NMP, stirred and coated on aluminum foil to make positive electrode sheet, and the negative electrode uses metal lithium sheet; the diaphragm is Celgard2400 polypropylene porous membrane; the solvent in the electrolyte is a solution composed of EC, DMC and EMC at a mass ratio of 1:1:1, the solute is LiPF6, and the concentration of LiPF6 is 1.0mol / L; 2023 button batteries are assembled in a glove box. The battery is tested for charge and discharge cycle performance, and the 0.2C discharge capacity is tested within the cut-off voltage range of 2.2 to 4.3V.
[0053] Embodiments 2 to 5
[0054] Examples 2 to 5 refer to the formula and method provided in Example 1 to prepare composite phosphoric acid material precursors, composite phosphoric acid materials, and batteries. The difference from Example 1 is that Examples 2 to 5 use the material of the water-soluble complexing agent, the pH of the metal solution, and the reaction temperature in S2 as variables, and the specific variables are shown in Table 2. In addition to the above differences, the operating steps for preparing composite phosphoric acid material precursors, composite phosphoric acid materials, and batteries in this example are strictly consistent with those in Example 1.
[0055] Table 2. Variables of Examples 2 to 5
[0056]
[0057] Example 6
[0058] This embodiment prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery with reference to the formula and method provided in Embodiment 1. The difference from Embodiment 1 is that the metal solutions used in this embodiment are metal solution A, metal solution C, and metal solution F (the addition time, reaction temperature, and pH are strictly consistent with those in Embodiment 1), wherein metal solution B, metal solution D, and metal solution E are replaced by metal solution C with equal mass fractions. Except for the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this embodiment are strictly consistent with those in Embodiment 1.
[0059] Example 7
[0060] This embodiment prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery with reference to the formula and method provided in Embodiment 1. The difference from Embodiment 1 is that the order of adding the metal solutions in this embodiment is metal solution A, metal solution E, metal solution D, metal solution C, metal solution B, and metal solution F. Except for the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this embodiment are strictly consistent with those in Embodiment 1.
[0061] Example 8
[0062] This example prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery with reference to the formula and method provided in Example 1. The difference from Example 1 is that this example uses the molar ratio of the Fe element, the Mn element, and the water-soluble chelating agent in the metal solution as variables, as shown in Table 3. Except for the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this example are strictly consistent with those in Example 1.
[0063] Table 3. Proportional relationship of each metal solution in Example 8
[0064] Components Raw material composition Metal solution A Fe element: Mn element: water-soluble complexing agent = 0:2:5 Metal solution B Fe element: Mn element: water-soluble complexing agent = 3:7:1 Metal solution C Fe element: Mn element: water-soluble complexing agent = 5:5:2 Metal solution D Fe element: Mn element: water-soluble complexing agent = 7:3:3 Metal solution E Fe element: Mn element: water-soluble complexing agent = 9:1:4 Metal solution F Fe element: Mn element: water-soluble complexing agent = 10:0:3
[0065] Example 9
[0066] This example prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery with reference to the formula and method provided in Example 1. The difference from Example 1 is that the pH of the metal solution is 6. Apart from the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this example are strictly consistent with those in Example 1.
[0067] Example 10
[0068] This example prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery with reference to the formula and method provided in Example 1. The difference from Example 1 is that the reaction temperature of the metal solution is 20°C. Apart from the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this example are strictly consistent with those in Example 1.
[0069] Comparative Example 1
[0070] This comparative example prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery with reference to the formula and method provided in Example 1. The difference from Example 1 is that this comparative example respectively configures Fe solution, Mn solution, and water-soluble complexing agent solution to replace the metal solution (keeping the total molar amount of each material unchanged). In addition to the above differences, the operation steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this comparative example are strictly consistent with those in Example 1. Specifically, the method for preparing this comparative example is:
[0071] S1. Prepare the base solution, Fe solution, Mn solution, complexing agent solution and phosphate solution respectively according to Table 1;
[0072] S2. In an inert gas atmosphere, e solution, Mn solution and complexing agent solution, phosphate solution and pH adjusting agent are added to the bottom liquid in parallel;
[0073] Steps S3 to S4 are strictly consistent with steps S3 to S4 provided in Example 1.
[0074] Comparative Example 2
[0075] This comparative example prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery by referring to the formula and method provided in Example 1. The difference from Example 1 is that no water-soluble chelating agent is added in this comparative example. Apart from the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this comparative example are strictly consistent with those in Example 1.
[0076] Comparative Example 3
[0077] This comparative example prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery with reference to the formula and method provided in Example 1. The difference from Example 1 is that this comparative example does not adjust the pH in step S3. Apart from the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this comparative example are strictly consistent with those in Example 1.
[0078] Comparative Example 4
[0079] This comparative example prepares a composite phosphoric acid material precursor, a composite phosphoric acid material, and a battery by referring to the formula and method provided in Example 1. The difference from Example 1 is that this comparative example does not perform aging treatment in step S3. Apart from the above differences, the operating steps for preparing the composite phosphoric acid material precursor, the composite phosphoric acid material, and the battery in this comparative example are strictly consistent with those in Example 1.
[0080] Comparative Example 5
[0081] This comparative example prepares a battery with reference to the formula and method provided in Example 1. The difference from Example 1 is that in the positive electrode prepared in this comparative example, the composite phosphoric acid material is replaced by an equal mass fraction of lithium iron manganese phosphate material. Except for the above difference, the operation steps for preparing the battery in this comparative example are strictly consistent with those in Example 1.
[0082] Comparative Example 6
[0083] This comparative example prepares a battery with reference to the formula and method provided in Example 1. The difference from Example 1 is that in the positive electrode prepared in this comparative example, the composite phosphoric acid material is replaced by lithium iron phosphate material with an equal mass fraction. Except for the above difference, the operation steps for preparing the battery in this comparative example are strictly consistent with those in Example 1.
[0084] Test Case
[0085] 1. Test subjects
[0086] The composite phosphoric acid materials prepared in Examples 1 to 10 and Comparative Examples 1 to 6 and the batteries using the same.
[0087] 2. Test Method
[0088] (1) Manganese dissolution: Weigh 2 portions of electrode materials of about 5g each as test objects and mark them. Dissolve the weighed test objects in 100ml of pure water, seal them, and let them stand for 70h. After filtering the test objects, dilute them in a 100ml volumetric flask, transfer 10ml of the test solution to a 100ml volumetric flask, add pure water to dilute, and shake well. Determine the concentration of the filtered solution using inductively coupled plasma emission spectrometry and calculate the results.
[0089] (2) Cycle performance: At 25°C, 1C rate, and 2.2-4.3V test conditions, the battery is charged and discharged for 500 cycles, and the cycle efficiency is measured.
[0090] (3) Low temperature performance: The battery is charged and discharged at -5°C, 1C rate, and 2.2 to 4.3V to obtain the low temperature performance of the battery.
[0091] 3. Result testing and analysis
[0092] The experimental data of this test case is shown in Table 4.
[0093] It can be seen from Examples 1 to 5 that different water-soluble complexing agents have different optimal reaction temperatures and complexing pH values. Moreover, different water-soluble complexing agents will affect the performance of the prepared composite phosphoric acid material and the battery using the composite phosphoric acid material, which may be due to the residual ligands participating in the calcination reaction, thereby affecting the structure of the composite phosphoric acid material.
[0094] In Examples 6 to 8, the effects of different ratios or types of metal solutions on the prepared composite phosphoric acid materials and applied batteries are explored. It can be seen from Example 6 that when the types of metal solutions are small, the composite phosphoric acid material formed can maintain a gradient concentration distribution with a gradually decreasing Mn content extending from the core to the shell, but the boundary is more obvious, which reduces the rate performance.
[0095] In Example 7, since the metal solutions were not introduced in the order of increasing molar content of the iron element, the Mn element in the prepared composite phosphate material did not show a gradient distribution, nor did the Mn element content gradually decrease from the inner core to the outer shell, resulting in a decrease in the cycle performance, rate performance and low-temperature performance of the battery using the composite phosphate material.
[0096] In Example 8, it can be found that when the ratio of Fe element, Mn element and water-soluble complexing agent in different metal solvents changes, the performance of the prepared composite phosphoric acid material also changes accordingly.
[0097] Combining Example 1 and Examples 9 to 10, it can be seen that when the pH and reaction temperature in the metal solution are both within a preferred range, the structure of the phosphorus-deficient ferromanganese phosphate precipitate formed is relatively stable, which helps to improve the dissolution of Mn ions.
[0098] In Comparative Example 1, only a single Fe solution, Mn solution and aqueous complexing agent solution are configured. Although the contents of Fe, Mn elements and complexing agents are reduced during the preparation process, since the reaction pH is a constant value, the Fe and Mn contents in the amorphous phosphorus-deficient ferromanganese phosphate precipitate formed are relatively fixed, and it is difficult to form a composite phosphoric acid material precursor in which the Mn element content gradually decreases from the inner core to the outer shell. From the tests in Comparative Examples 2 to 4, it can be seen that whether it is the lack of a water-soluble complexing agent or the lack of a certain treatment step (such as not adjusting the pH or not performing an aging treatment), the electrochemical performance of the battery using it will be significantly reduced.
[0099] It can be seen from the data of Example 1 and Comparative Examples 5 to 6 that the composite phosphate material provided by the present invention can significantly improve the problem of manganese dissolution, and provide a material having good cycle performance, rate performance and low temperature performance.
[0100] Table 4. Test results of this test case
[0101]
[0102]
[0103] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a composite phosphoric acid material precursor, It is characterized in that The preparation method comprises the following steps: S1. Prepare a base solution, a metal solution, and a phosphate solution respectively, wherein the base solution is an ammonia solution with a concentration of 1 to 8 g / L; the metal solution includes at least one of a metal element and a water-soluble complexing agent, and the metal element includes at least one of an Fe element and a Mn element; in the metal solution, the molar ratio of Fe element: Mn element: the water-soluble complexing agent is 0 to 10: 0 to 8: 0 to 5; S2. In an inert gas atmosphere, the metal solution, the phosphate solution and the pH adjuster are added to the bottom liquid in parallel; S3. The pH of the reaction system was adjusted to 4 to 9, and then the liquid was stopped and aged; S4. Performing solid-liquid separation on the reaction solution, and calcining the obtained solid under an inert gas atmosphere to obtain the composite phosphoric acid material precursor.
2. The method for preparing the composite phosphoric acid material precursor according to claim 1, It is characterized in that The metal solution is prepared by at least one of the water-soluble complexing agent, the water-soluble iron source, and the water-soluble manganese source; Wherein, the water-soluble iron source includes at least one of ferrous sulfate, ferric sulfate, ferric nitrate and ferric chloride, and / or the water-soluble manganese source includes at least one of manganese sulfate, manganese nitrate, manganese chloride and manganese acetate.
3. The method for preparing the composite phosphoric acid material precursor according to claim 1, It is characterized in that In the metal solution, the molar amount of the water-soluble complexing agent is 10-50% of the total molar amount of the iron element, and the water-soluble complexing agent includes at least one of ethylenediaminetetraacetic acid, potassium thiocyanate, sodium citrate and vitamin C.
4. The method for preparing the composite phosphoric acid material precursor according to claim 3, It is characterized in that The metal solution includes at least one of metal solution A, metal solution B, metal solution C, metal solution D, metal solution E, and metal solution F; Wherein, in the metal solution A, the molar ratio of Fe element: Mn element: water-soluble complexing agent is 0:1:0; In the metal solution B, the molar ratio of Fe element: Mn element: water-soluble complexing agent is 2:8:1; In the metal solution C, the molar ratio of Fe element: Mn element: water-soluble complexing agent is 4:6:2; In the metal solution D, the molar ratio of Fe element: Mn element: water-soluble complexing agent is 6:4:3; In the metal solution E, the molar ratio of Fe element: Mn element: water-soluble complexing agent is 8:2:4; In the metal solution F, calculated by molar ratio, Fe element: Mn element: water-soluble complexing agent = 10:0:
5.
5. The method for preparing the composite phosphoric acid material precursor according to claim 4, It is characterized in that In S2, the metal solution includes the metal solution A, the metal solution F, and also includes at least one of the metal solution B, the metal solution C, the metal solution D, and the metal solution E; the added metal solutions are replaced in sequence at intervals of 20 to 120 minutes in the order of increasing molar content of the iron element.
6. The method for preparing the composite phosphoric acid material precursor according to any one of claims 1 to 5, It is characterized in that In the metal solution, the water-soluble complexing agent is ethylenediaminetetraacetic acid, and the pH of the metal solution is 2-10. The reaction temperature of the reaction system in S2 is 30-90°C.
7. The method for preparing the composite phosphoric acid material precursor according to any one of claims 1 to 5, It is characterized in that The water-soluble complexing agent is potassium thiocyanate, the pH of the metal solution is 4-10, and the reaction temperature of the reaction system in S2 is 40-80°C.
8. The method for preparing the composite phosphoric acid material precursor according to any one of claims 1 to 5, It is characterized in that The water-soluble complexing agent is sodium citrate, and the pH of the metal solution is 3-10. The reaction temperature of the reaction system in S2 is 50-90°C.
9. A composite phosphoric acid material, It is characterized in that The composite phosphoric acid material is prepared by calcining a lithium source and a composite phosphoric acid material precursor, and the composite phosphoric acid material precursor is prepared by the preparation method of the composite phosphoric acid material precursor according to any one of claims 1 to 8.
10. An electrode, It is characterized in that The electrode comprises the composite phosphoric acid material as claimed in claim 9.
11. A battery, It is characterized in that The battery comprises the electrode as claimed in claim 10.
Citation Information
Patent Citations
Sodium-ion battery quaternary positive electrode material precursor and preparation method and application thereof
CN115594233A
Ferric manganese phosphate precursor, lithium iron manganese phosphate positive electrode material and preparation method and application of ferric manganese phosphate precursor and lithium iron manganese phosphate positive electrode material
CN118083937A
Preparation method of ammonium manganese iron phosphate precursor and lithium manganese iron phosphate
CN118164461A