Preparation method of pomegranate peel derived hard carbon material and application of pomegranate peel derived hard carbon material in sodium ion battery
Through simple pyrolysis and acid treatment methods, pomegranate peels are used to prepare new hard carbon materials, which solves the high cost and environmental problems of sodium-ion battery anode materials and realizes high-performance sodium-ion battery materials with excellent electrochemical properties and environmental protection. economic advantage.
Patent Information
- Application Number
- CN202411000310.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
AI Technical Summary
Existing sodium-ion battery anode materials have high cost, heavy environmental burden, and insufficient electrochemical performance. In particular, they rely on petrochemical by-products in the preparation process of hard carbon materials, leading to environmental protection and performance problems.
Through simple pyrolysis and acid treatment methods, biomass waste pomegranate peels were used to prepare new hard carbon materials. The pyrolysis process parameters and acid treatment process were optimized to regulate the structure and performance of the material, and pomegranate peels with excellent electrochemical properties were prepared. Derived hard carbon materials.
It achieves efficient sodium ion storage capacity and good cycle stability and rate performance, significantly improves the overall performance of sodium ion batteries, has environmental protection and economic advantages, and provides an innovative strategy for the resource utilization of biomass resources.
Smart Images

Figure CN118754101A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of secondary batteries, and specifically to a method for preparing a novel hard carbon material for a negative electrode of a sodium ion battery, wherein the hard carbon material with excellent electrochemical properties is obtained by simply pyrolyzing and acid-treating biomass waste pomegranate peel. Background Art
[0002] In recent years, sodium-ion batteries have attracted widespread attention as a potential energy storage technology to replace lithium-ion batteries. Compared with lithium, sodium is more abundant, cheaper, and widely distributed, which can reduce dependence on lithium resources in specific regions. However, sodium-ion batteries still face many challenges in practical applications, especially in the selection of negative electrode materials and performance optimization.
[0003] Existing negative electrode materials include hard carbon, soft carbon, metal oxides, alloys, etc. Among them, hard carbon materials have attracted much attention due to their superior electrochemical performance and cycle stability. Hard carbon materials have a disordered layered structure, which can provide a large interlayer spacing, which is conducive to the insertion and deintercalation of sodium ions. However, the traditional preparation process of hard carbon materials usually relies on petrochemical by-products or synthetic precursors, which not only increases costs but also imposes a burden on the environment.
[0004] Therefore, finding a low-cost, environmentally friendly and high-performance hard carbon material preparation method has become a research hotspot. In recent years, the research on biomass waste as a precursor of hard carbon materials has gradually increased. Biomass resources are abundant, inexpensive and renewable. Hard carbon materials with good electrochemical properties can be obtained through pyrolysis treatment. At the same time, the use of biomass waste to prepare hard carbon materials also has the advantages of environmental friendliness and resource recycling.
[0005] Among many biomass resources, pomegranate peel is a common agricultural waste with high carbon content and rich microporous structure, making it an ideal precursor for preparing hard carbon materials. However, the current research on pomegranate peel-derived hard carbon materials is still relatively limited, and most of them focus on simple pyrolysis processes. The research on its structure regulation and electrochemical performance optimization has not been carried out in depth.
[0006] In addition, the electrochemical performance of hard carbon materials depends largely on their microstructure and surface chemical properties. For example, the size of the interlayer spacing, specific surface area, pore structure, and the presence of surface functional groups will affect the storage and transport performance of sodium ions. Therefore, by optimizing the pyrolysis process parameters and post-treatment process, the structure and properties of hard carbon materials can be effectively regulated.
[0007] Based on the above background, the present invention proposes a method for preparing a new hard carbon material using biomass waste pomegranate peel as a precursor through a simple pyrolysis method combined with acid treatment. By systematically studying the effects of different carbonization temperatures on the morphology and structure of pomegranate peel-derived hard carbon materials, the optimal preparation conditions were optimized, and the application performance of the material in the negative electrode of sodium ion batteries was further explored. The research results show that the new hard carbon material has an enlarged interlayer spacing and improved ion transport characteristics, and exhibits excellent electrochemical properties. It not only provides new ideas for the development of high-performance sodium ion battery negative electrode materials, but also provides an important reference for the resource utilization of biomass waste. Summary of the invention
[0008] The purpose of the present invention is to prepare a new hard carbon material (PPHC) using biomass waste pomegranate peel as a precursor through a simple pyrolysis method combined with acid treatment to solve the problems of high cost, heavy environmental burden and insufficient electrochemical performance of existing sodium ion battery negative electrode materials. The prepared PPHC material can not only provide efficient sodium ion storage capacity, but also has good cycle stability and rate performance, thereby improving the overall performance of sodium ion batteries.
[0009] In order to achieve the above object, the present invention proposes a technical solution for preparing a hard carbon material, comprising the following steps:
[0010] S1 Raw material processing: pomegranate peel was cut into small pieces, thoroughly washed with deionized water and ethanol under ultrasonic assistance, and dried;
[0011] S2 Pyrolysis: The dried pomegranate peel was pyrolyzed in a tube furnace (temperature of 1100°C to 1300°C) for 2 hours at a heating rate of 3°C / min under argon protection;
[0012] S3 acid treatment: washing the prepared raw carbon material with hydrochloric acid and hydrofluoric acid at 60°C to remove inorganic impurities;
[0013] Preferably, in step S1, the pomegranate peel cleaning process is performed with the assistance of ultrasound to improve the cleaning efficiency.
[0014] Preferably, in step S2, the pyrolysis process is carried out in a tubular furnace, the pyrolysis temperature range is 1100° C. to 1300° C., and the pyrolysis time is 2 hours.
[0015] Preferably, in step S2, the pyrolysis process is carried out under argon protection to prevent oxidation of the material.
[0016] Preferably, in step S3, during the acid treatment process, the material is first cleaned with hydrochloric acid having a material to acid ratio of 1:10, and then cleaned with hydrofluoric acid having a material to acid ratio of 1:5.
[0017] Preferably, in step S3, the hard carbon material (PPHC) has a large interlayer spacing, appropriate carboxyl groups and a low specific surface area.
[0018] A new type of hard carbon material derived from pomegranate peel is prepared by the above method; the hard carbon material (PPHC) exhibits a high performance of 330 mAhg -1 The reversible capacity is maintained at 174 mAh g at 1 C current rate. -1 , after 200 cycles at 0.5C, the capacity is 175 mAh g -1 .
[0019] The above-mentioned new type of hard carbon material derived from pomegranate peel is used in sodium ion batteries.
[0020] The hard carbon material (PPHC) prepared by the present invention has the following beneficial effects:
[0021] 1. Excellent electrochemical performance: As a negative electrode material for sodium-ion batteries, PPHC exhibits a reversible capacity of up to 330 mAh g-1. It can still maintain a high capacity under high rate and long cycle conditions, significantly improving the overall performance of sodium-ion batteries.
[0022] 2. Structural advantages: PPHC materials have an enlarged interlayer spacing and a lower specific surface area, which is conducive to the embedding and deintercalation of sodium ions, thereby improving the capacity and rate performance of the battery.
[0023] 3. Environmental protection and economy: Using biological waste pomegranate peel as a precursor, the preparation process is simple and low-cost, while effectively utilizing agricultural waste, which has important environmental and economic significance.
[0024] 4. Process optimization: By optimizing the pyrolysis process parameters and acid treatment process, the structure and properties of hard carbon materials can be precisely controlled, providing a technical basis for large-scale production.
[0025] The present invention not only provides a new idea for the development of high-performance sodium-ion battery negative electrode materials, but also provides an innovative strategy for the resource utilization of biomass waste, and has broad application prospects and important social value. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0027] Figure 1It is a schematic diagram of the preparation process of the pomegranate peel derived hard carbon material (PPHC) in the present invention;
[0028] Figure 2 These are the rate performance test results of the materials obtained in Comparative Examples 1 to 3 and Examples 1 to 3 of the present invention;
[0029] Figure 3 These are the cycle performance test results of the materials obtained in Comparative Examples 1 to 3 and Examples 1 to 3 of the present invention;
[0030] Figure 4 These are the impedance performance test results of the materials obtained in Comparative Examples 1 to 3 and Examples 1 to 3 of the present invention;
[0031] Figure 5 These are SEM and TEM images of the materials obtained in Comparative Examples 1 to 3 and Examples 1 to 3 of the present invention. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0033] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0034] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions).
[0035] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0036] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0037] like Figure 1 As shown, the present invention provides a method for preparing a novel sodium ion battery negative electrode hard carbon material derived from pomegranate peel, comprising the following steps:
[0038] S1: The pomegranate peel was cut into small pieces of about 1 to 2 cm in size; and the pieces were thoroughly washed with deionized water and ethanol under the assistance of ultrasonic wave; and then dried in a vacuum oven at 100° C. overnight.
[0039] The pomegranate peels were sourced from pomegranate products purchased in a local fruit market (Xi’an, Shaanxi Province, China).
[0040] S2: The dried pomegranate peel is pyrolyzed in a tube furnace for 2 hours; in this step, the temperature of the tube furnace is increased at a rate of 3°C / min to 1100°C to 1300°C; and the process is carried out under argon protection.
[0041] S3: The prepared raw carbon material was then washed with hydrochloric acid (material: acid = 1:10) and hydrofluoric acid (material: acid = 1:5) at 60°C for 3 hours to remove inorganic impurities.
[0042] A new type of sodium ion battery negative electrode hard carbon material (PPHC) derived from pomegranate peel is prepared by the above method; the hard carbon material (PPHC) exhibits a high performance of up to 330 mAhg -1 The reversible capacity is maintained at 174 mAh g at 1 C current rate. -1 ; After 200 cycles at 0.5C, the capacity of PPHC is 175 mAh g -1 .
[0043] The above-mentioned new type of sodium ion battery negative electrode hard carbon material (PPHC) derived from pomegranate peel is used in sodium ion batteries.
[0044] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0045] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0046] The pomegranate peels used in the embodiments and comparative examples were all from pomegranate products purchased from the fruit market in Xi'an, Shaanxi Province, China.
[0047] Comparative Example 1
[0048] (1) Cut the pomegranate peel into small pieces of about 1 to 2 cm in size; wash them thoroughly with deionized water and ethanol under ultrasonic assistance; and then dry them in a vacuum oven at 100° C. overnight;
[0049] (2) Under argon protection, the dried pomegranate peel was heated to 1100°C at a rate of 3°C / min in a tube furnace for pyrolysis for 2 hours to obtain a hard carbon material.
[0050] Comparative Example 2
[0051] (1) Cut the pomegranate peel into small pieces of about 1 to 2 cm in size, and wash them thoroughly with deionized water and ethanol under ultrasonic assistance; then dry them in a vacuum oven at 100° C. overnight.
[0052] (2) The dried pomegranate peel is pyrolyzed in a tube furnace for 2 hours; in this step, the temperature of the tube furnace is increased at a rate of 3°C / min to 900°C; and the process is carried out under argon protection.
[0053] (3) The carbon material obtained in step (2) was washed with hydrochloric acid (material: acid = 1:10) and hydrofluoric acid (material: acid = 1:5) at 60°C for 3 hours to remove inorganic impurities.
[0054] Comparative Example 3
[0055] (1) Cut the pomegranate peel into small pieces of about 1 to 2 cm in size, and wash them thoroughly with deionized water and ethanol under ultrasonic assistance; then dry them in a vacuum oven at 100° C. overnight.
[0056] (2) The dried pomegranate peel is pyrolyzed in a tube furnace for 2 hours; in this step, the temperature of the tube furnace is increased at a rate of 3°C / min to 1000°C; and the process is carried out under argon protection.
[0057] (3) The carbon material obtained in step (2) was washed with hydrochloric acid (material: acid = 1:10) and hydrofluoric acid (material: acid = 1:5) at 60°C for 3 hours to remove inorganic impurities.
[0058] Example 1
[0059] (1) Cut the pomegranate peel into small pieces of about 1 to 2 cm in size, and wash them thoroughly with deionized water and ethanol under ultrasonic assistance; then dry them in a vacuum oven at 100° C. overnight.
[0060] (2) The dried pomegranate peel is pyrolyzed in a tube furnace for 2 hours; in this step, the temperature of the tube furnace is increased at a rate of 3°C / min to 1100°C; and the process is carried out under argon protection.
[0061] (3) The carbon material obtained in step (2) was washed with hydrochloric acid (material: acid = 1:10) and hydrofluoric acid (material: acid = 1:5) at 60°C for 3 hours to remove inorganic impurities.
[0062] Example 2
[0063] (1) Cut the pomegranate peel into small pieces of about 1 to 2 cm in size, and wash them thoroughly with deionized water and ethanol under ultrasonic assistance; then dry them in a vacuum oven at 100° C. overnight.
[0064] (2) The dried pomegranate peel is pyrolyzed in a tube furnace for 2 hours; in this step, the temperature of the tube furnace is increased at a rate of 3°C / min to 1200°C; and the process is carried out under argon protection.
[0065] (3) The carbon material obtained in step (2) was washed with hydrochloric acid (material: acid = 1:10) and hydrofluoric acid (material: acid = 1:5) at 60°C for 3 hours to remove inorganic impurities.
[0066] Example 3
[0067] (1) Cut the pomegranate peel into small pieces of about 1 to 2 cm in size, and wash them thoroughly with deionized water and ethanol under ultrasonic assistance; then dry them in a vacuum oven at 100° C. overnight.
[0068] (2) The dried pomegranate peel is pyrolyzed in a tube furnace for 2 hours; in this step, the temperature of the tube furnace is increased at a rate of 3°C / min to 1300°C; and the process is carried out under argon protection.
[0069] (3) The carbon material obtained in step (2) was washed with hydrochloric acid (material: acid = 1:10) and hydrofluoric acid (material: acid = 1:5) at 60°C for 3 hours to remove inorganic impurities.
[0070] The rate performance test results of the materials obtained in the above comparative examples 1 to 3 and embodiments 1 to 3 are shown in Figure 2 ,Depend on Figure 2 It can be seen that at a current density of 0.1C, the first reversible capacities of Comparative Example 1, Comparative Example 2, Comparative Example 3, Example 1, Example 2 and Example 3 can reach 505.5, 423.0, 438.6, 718.2, 513.1 and 542.3 mAh·g, respectively. -1After 35 cycles, when the current density returned to 0.1C, the reversible capacities of Comparative Example 1, Comparative Example 2, Comparative Example 3, Example 1, Example 2 and Example 3 were 241.9, 165.1, 176.5, 308.6, 261.4 and 267.2 mAh·g, respectively. -1 It can be seen that compared with the carbon materials obtained at lower pyrolysis temperatures (900°C and 1000°C) (Comparative Examples 2 and 3), the carbon materials obtained at a pyrolysis temperature > 1000°C have a higher specific capacity; and at the same pyrolysis temperature (1100°C), compared with the carbon material that has not undergone the acid washing step (Comparative Example 1), the carbon material that has undergone the acid washing step (Example 1) has a higher specific capacity.
[0071] At the same time, the cycle performance test results of the materials obtained in the above comparative examples 1 to 3 and embodiments 1 to 3 are shown in Figure 3 ,Depend on Figure 3 It can be seen that after 150 cycles at a current density of 0.5C, the reversible capacities of Comparative Example 1, Comparative Example 2, Comparative Example 3, Example 1, Example 2 and Example 3 are 91.7, 93.6, 108.5, 200.9, 145.8 and 123.8 mAh g, respectively. -1 It can be seen that the material obtained by pyrolysis at a higher temperature and acid washing in the present invention has better structural stability.
[0072] The impedance performance test results of the materials obtained in the above comparative examples 1 to 3 and embodiments 1 to 3 are shown in Figure 4 ,Depend on Figure 4 It can be seen that the high-frequency resistance of Comparative Example 1, Comparative Example 2, Comparative Example 3, Example 1, Example 2 and Example 3 are 164, 104, 103, 50, 61 and 83Ω respectively. It can be seen that compared with the carbon material that has not been acid-washed (Comparative Example 1) or the carbon material that has been pyrolyzed and acid-washed at a lower temperature (Comparative Examples 2 and 3), the carbon material that has been pyrolyzed and acid-washed at high temperature (Examples 1, 2, 3) has better conductivity.
[0073] The SEM and TEM images of the materials obtained in the above Comparative Examples 1 to 3 and Examples 1 to 3 are shown in Figure 5 ,Depend on Figure 5 It can be seen that larger particles can still be seen in the structures of Comparative Examples 2 and 3, which is not conducive to their sodium storage performance; while in Example 1, most of the biomass structure is decomposed, and new particles in the range of 5 to 10 microns are reconstructed. This corrugated surface and porous structure are conducive to the diffusion of sodium ions, thereby improving the electrochemical performance; and through TEM observations, it can be seen that the materials of Examples 1, 2, and 3 have a larger interlayer spacing.
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a hard carbon material suitable for a negative electrode of a sodium ion battery by using a pyrolysis method combined with an acid treatment, using a biomass waste pomegranate peel as a precursor, characterized in that: The following steps are involved: S1: Cut the pomegranate peel into small pieces, wash them with deionized water and ethanol under ultrasonic assistance, and then dry them in a vacuum oven; S2: Pyrolyzing the dried pomegranate peel at a temperature of 1100° C. to 1300° C. for 2 hours in a tube furnace at a heating rate of 3° C. / min and under argon protection; S3: The pyrolyzed carbon material was washed with hydrochloric acid (material: acid = 1:10) and hydrofluoric acid (material: acid = 1:5) at 60° C. for 3 hours to remove inorganic impurities and obtain a hard carbon material (PPHC).
2. The method according to claim 1, characterized in that In step S1, the pomegranate peel cleaning process is performed with the assistance of ultrasonic waves to improve the cleaning efficiency.
3. The method according to claim 1, characterized in that In step S2, the pyrolysis process is carried out in a tubular furnace, the pyrolysis temperature ranges from 1100° C. to 1300° C., and the pyrolysis time is 2 hours.
4. The method according to claim 1, characterized in that: In step S2, the pyrolysis process is carried out under argon protection to prevent oxidation of the material.
5. The method according to claim 1, characterized in that In step S3, during the acid treatment, the ratio of hydrochloric acid to hydrofluoric acid is 1:10 and 1:5 respectively.
6. The method according to claim 1, characterized in that In the step S3, the obtained hard carbon material (PPHC) has a larger interlayer distance, appropriate carboxyl groups and a lower specific surface area.
7. A hard carbon material (PPHC) prepared by the method according to any one of claims 1 to 6, characterized in that: It exhibits a reversible capacity of up to 330 mAh g-1 in the sodium-ion battery anode and maintains 174 mAh g-1 at a current rate of 1C. The capacity is 175 mAh g-1 after 200 cycles at 0.5C.
8. Use of a novel hard carbon material derived from pomegranate peel (PPHC) as described in the claim in sodium ion batteries.
Citation Information
Patent Citations
Pyrolytic hard carbon material and application thereof
CN106185862A
A preparation method of biomass hard carbon material for negative electrode of sodium ion battery
CN109004199A
Cattle manure derived hard carbon as electrode material for sodium ion batteries and
IN202011048103A