Coal-based carbon negative electrode material for sodium-ion battery as well as preparation method and application of coal-based carbon negative electrode material

Through heterogeneous crosslinking treatment of theabaoxin and bituminous coal, the preparation process of coal-based carbon materials is simplified, the problems of excessive oxygen and process complexity in the introduction of oxidative reagents in the prior art are solved, and the storage of sodium ion battery negative electrode materials is improved Sodium performance and first-time Coulomb efficiency.

CN119038519AActive Publication Date: 2024-11-29NORTHEASTERN UNIV AT QINHUANGDAO

Patent Information

Application Number
CN202411019009.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-29
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

In the prior art, when preparing coal-based carbon anode material for sodium ion batteries, the strong oxidizing reagent introduces excessive oxygen elements, which takes a long time, is complex in the process and is costly, which affects the sodium storage performance of the material.

Method used

Theodonin and bituminous coal are mixed with and pre-oxidized under a low-temperature oxygen atmosphere to form a heterogeneous crosslinked structure, hindering the growth of graphite microcrystals, and coal-based carbon materials with high capacity and first-time Coulomb efficiency are obtained through high-temperature carbonization.

Benefits of technology

The process is simplified, the cost is reduced, the amorphous structure and layer spacing of coal-based carbon materials are improved, and the storage capacity of sodium ions is enhanced. The first time the Coulomb efficiency reaches more than 73%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038519A_ABST
    Figure CN119038519A_ABST
Patent Text Reader

Abstract

The invention provides a coal-based carbon negative electrode material for a sodium ion battery as well as a preparation method and application of the coal-based carbon negative electrode material. The method provided by the invention comprises the following steps: (1) soaking bituminous coal in a mixed acid solution containing hydrochloric acid and hydrofluoric acid, washing until the solution is neutral, and then drying to obtain dry pulverized coal; (2) mixing theabrownin with dry pulverized coal, and performing pre-oxidation treatment in an oxygen-containing atmosphere to obtain a pre-oxidation product; and (3) carbonizing the pre-oxidized product in an inert atmosphere so as to obtain the coal-based carbon material. The coal-based carbon material can be used as a sodium ion battery negative electrode, and has high capacity and first coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of energy storage hard carbon materials, and specifically relates to a coal-based carbon negative electrode material for sodium ion batteries and a preparation method and application thereof. Background Art

[0002] The shortage of lithium resources has restricted the further development of lithium-ion batteries in the field of large-scale energy storage. my country is rich in sodium resources, and sodium and lithium have similar chemical properties. Sodium-ion batteries have become a powerful alternative to lithium-ion batteries. Among the negative electrode materials of sodium-ion batteries, hard carbon is the most commercially promising sodium storage negative electrode material. Bituminous coal resources are abundant, low cost, and high carbon yield. Therefore, bituminous coal-based hard carbon is a very promising negative electrode material for sodium-ion batteries.

[0003] However, bituminous coal is a polycyclic aromatic hydrocarbon macromolecular structure, which contains basic structural units composed of aromatic rings, fatty side chains and functional groups. During the pyrolysis process, the condensation of aromatic rings easily causes the growth of graphite crystallites and the increase of graphitization degree, which is not conducive to the storage of sodium ions.

[0004] The Chinese patent application with publication number CN114335522A records that coal-based materials are oxidized by oxidizing agents such as sulfur-containing reagents, then mixed with volatile organic matter, then subjected to low-temperature heat treatment, and finally subjected to high-temperature heat treatment to obtain coal-based carbon negative electrode materials. However, this design process introduces excessive oxygen elements through pre-oxidation treatment with strong oxidizing agents, resulting in a significant carbonization yield of coal, and involves low-temperature pyrolysis and coating of volatile organic matter, which is time-consuming and not conducive to large-scale development and application.

[0005] The Chinese patent application with publication number CN115784196A records that coal is pretreated in an oxygen-containing atmosphere, and then the pretreated coal and the combined treatment agent are pre-calcined in the first stage, and then calcined in the second stage under negative pressure to obtain a coal-based sodium ion battery carbon negative electrode material. This method is complex and uses combined treatment agents such as ammonium salts and transition metal salts, which is costly.

[0006] The Chinese patent application with publication number CN117105198A records that coal and inorganic salt are mixed, ball-milled in an oxygen-containing atmosphere, and then the inorganic salt in the mixture is removed to obtain a coal-based precursor; the coal-based precursor is carbonized to obtain the coal-based carbon material. This method also uses inorganic salts, which need to be removed, and has high costs and a complicated process.

[0007] The preparation methods of coal-based carbon materials need to be further optimized. Summary of the invention

[0008] The present invention aims to solve one of the technical problems in the related art at least to a certain extent.

[0009] In view of the above-mentioned technical deficiencies, the present invention provides a coal-based carbon negative electrode material for sodium ion batteries, a preparation method and an application thereof. Theabrownin is a natural high-polymer complex extracted from Pu'er tea, and its surface is rich in functional groups such as carboxyl and hydroxyl groups. When bituminous coal and theabrownin are mixed, in an atmosphere of low-temperature oxygen, the oxygen-containing functional groups on the surface of the coal and the oxygen-containing functional groups of theabrownin undergo heterogeneous cross-linking, and the cross-linking structure can hinder the growth of graphite crystallites during the subsequent pyrolysis process, forming a coal-based carbon amorphous structure that is conducive to the storage of sodium ions. The provided coal-based carbon material can be used to prepare the negative electrode of a sodium ion battery, and has a high capacity and first coulombic efficiency.

[0010] To achieve the above object, the present invention provides the following technical solutions:

[0011] A first aspect of the present invention provides a method for preparing a coal-based carbon negative electrode material for a sodium ion battery, comprising the following steps:

[0012] (1) soaking the bituminous coal in a mixed acid solution containing hydrochloric acid and hydrofluoric acid, rinsing until the solution is neutral, and then drying to obtain dry coal powder;

[0013] (2) mixing the theabrownin with the dry coal powder obtained in step (1), and performing a pre-oxidation treatment in an oxygen-containing atmosphere to obtain a pre-oxidation product;

[0014] (3) carbonizing the pre-oxidation product under an inert atmosphere to obtain a coal-based carbon material;

[0015] According to an embodiment of the present invention, the bituminous coal in step (1) is pre-crushed, and the particle size of the crushed bituminous coal is 45 microns to 74 microns.

[0016] According to an embodiment of the present invention, the volume ratio of hydrochloric acid to hydrofluoric acid in the mixed acid solution containing hydrochloric acid and hydrofluoric acid in step (1) is (1-4):(1-4).

[0017] According to an embodiment of the present invention, the soaking treatment time in step (1) is 5 to 48 hours.

[0018] According to an embodiment of the present invention, the mass ratio of theabrownin to dry coal powder in step (2) is (1-6):(1-6).

[0019] According to an embodiment of the present invention, the oxygen-containing atmosphere in step (2) is selected from at least one of air and oxygen.

[0020] According to an embodiment of the present invention, the inert atmosphere in step (3) is at least one of argon, nitrogen and helium.

[0021] According to an embodiment of the present invention, the temperature of the pre-oxidation treatment in step (2) is 200-400°C.

[0022] According to an embodiment of the present invention, the time of the pre-oxidation treatment in step (2) is 1-12 hours.

[0023] According to an embodiment of the present invention, the carbonization temperature in step (3) is 1200-1700°C.

[0024] According to an embodiment of the present invention, the carbonization time in step (3) is 1 to 4 hours.

[0025] According to an embodiment of the present invention, the heating rate of the carbonization in step (3) is 1 to 10° C. / min.

[0026] In a second aspect of the present invention, a coal-based carbon negative electrode material for a sodium ion battery is provided, which is prepared by the preparation method described in any embodiment of the first aspect.

[0027] In a third aspect of the present invention, a sodium ion battery negative electrode is provided, comprising the coal-based carbon negative electrode material for a sodium ion battery according to the second aspect.

[0028] The beneficial effects achieved by the present invention include at least:

[0029] The present invention creatively uses theabrownin containing oxygen functional groups as a regulating agent, inhibits the growth of graphite microcrystals through heterogeneous cross-linking, improves the amorphous degree and interlayer spacing of carbon materials, and is suitable for the storage of sodium ions.

[0030] The method for preparing the coal-based carbon material provided by the present invention is simple and easy to industrially produce. Through the subsequent high-temperature treatment, the twisted graphite crystallites are rearranged to form a closed-pore structure, thereby improving the first coulombic efficiency of coal-based carbon sodium storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the XRD pattern of the coal-based carbon material for the sodium ion battery negative electrode prepared in Example 1.

[0032] Figure 2 This is a scanning electron microscope image of the coal-based carbon material for the sodium ion battery negative electrode prepared in Example 1.

[0033] Figure 3 This is the XRD pattern of the coal-based carbon material for the sodium ion battery negative electrode prepared in Example 2.

[0034] Figure 4 This is a scanning electron microscope image of the coal-based carbon material for the sodium ion battery negative electrode prepared in Example 2.

[0035] Figure 5This is the XRD pattern of the coal-based carbon material for the sodium ion battery negative electrode prepared in Example 3.

[0036] Figure 6 This is a scanning electron microscope image of the coal-based carbon material for the negative electrode of the sodium ion battery prepared in Example 3.

[0037] Figure 7 This is the XRD pattern of the coal-based carbon material for the sodium ion battery negative electrode prepared in Example 4.

[0038] Figure 8 This is a scanning electron microscope image of the coal-based carbon material for the sodium ion battery negative electrode prepared in Example 4.

[0039] Fig. 9 This is the XRD diagram of the coal-based carbon material for the sodium ion battery negative electrode prepared in Comparative Example 1.

[0040] Fig.10 This is a scanning electron microscope image of the coal-based carbon material for the negative electrode of the sodium ion battery prepared in Comparative Example 1.

[0041] Fig.11 This is the XRD diagram of the coal-based carbon material for the sodium ion battery negative electrode prepared in Comparative Example 2.

[0042] Fig.12 This is a scanning electron microscope image of the coal-based carbon material for the negative electrode of the sodium ion battery prepared in Comparative Example 2. DETAILED DESCRIPTION

[0043] Embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0044] The present invention provides a method for preparing a coal-based carbon negative electrode material for a sodium ion battery, comprising:

[0045] (1) soaking in a mixed acid solution containing hydrochloric acid and hydrofluoric acid, rinsing until the solution is neutral, and then drying to obtain dry coal powder;

[0046] (2) mixing the theabrownin with the dry coal powder obtained in step (1), and performing a pre-oxidation treatment in an oxygen-containing atmosphere to obtain a pre-oxidation product;

[0047] (3) Carbonizing the pre-oxidation product under an inert atmosphere to obtain a coal-based carbon material.

[0048] After the bituminous coal is crushed, it is acid-washed to remove organic minerals in the coal. The acid-washed coal is mixed with the regulating agent theabrownin and pre-oxidized in an oxygen-containing atmosphere; the pre-oxidation product is carbonized at high temperature to prepare a coal-based carbon material suitable for the negative electrode of a sodium ion battery. Theabrownin contains abundant oxygen-containing functional groups. Through low-temperature pre-oxidation, it constructs a heterogeneous cross-linked structure with the oxygen functional groups on the surface of the bituminous coal, hinders the lateral growth and longitudinal stacking of carbon microcrystals, regulates the degree of disordered arrangement of microcrystals, and obtains an amorphous hard carbon material with a large interlayer spacing and rich closed-pore structure. The obtained coal-based material has high capacity and first coulomb efficiency when used as the negative electrode of a carbon sodium ion battery. The first coulomb efficiency is above 73%, preferably above 75%; the first discharge specific capacity is above 420mAh / g, preferably above 440mAh / g.

[0049] The bituminous coal mentioned in this article is a kind of coal with a medium coalification degree, a carbon content of 80% to 90%, a hydrogen content of 4% to 6%, and an oxygen content of 10% to 15%. Bituminous coal has a range of metamorphic degrees, and the bituminous coal mentioned in this article includes bituminous coal of all metamorphic degrees. The bituminous coal can be pulverized in advance, and the pulverization used can adopt the technology and equipment known in the art, preferably using pulverization equipment, such as one or more of air flow pulverization, roller mill, mechanical mill, and ball mill.

[0050] According to a specific embodiment, the volume ratio of hydrochloric acid to hydrofluoric acid in the provided mixed acid solution is 1 to 4:1 to 4. The time for the mixed acid soaking treatment is 5 to 48 hours.

[0051] When the theabrownin is mixed with dry coal powder, mechanical equipment with high shear force commonly used in the art can be used, such as a fusion machine or a kneading machine, etc. According to a specific embodiment, the mixing mass ratio of the theabrownin and the dry coal powder is 1-10:1-10. According to a preferred embodiment, the mixing ratio of the theabrownin and the dry coal powder is 1-6:1-6. According to a preferred embodiment, the mixing ratio of the theabrownin and the dry coal powder is (1-2):(2-5), for example, (1-1.5):(2.5-5).

[0052] The oxygen-containing atmosphere mentioned may refer to one or more of air, oxygen and ozone, such as air, for convenience and cost control. The oxygen content of the oxygen-containing atmosphere mentioned may be 20% to 100%. According to a specific embodiment, the oxygen-containing atmosphere used in the pre-oxidation treatment includes air and pure oxygen, the pre-oxidation temperature is 200 to 400°C (270 to 350 degrees Celsius according to a preferred embodiment), and the pre-oxidation time is 1-12h (6 to 12 hours according to a preferred embodiment).

[0053] According to a specific implementation manner, the inert atmosphere used in the carbonization of the pre-oxidation product is any one of argon, nitrogen, helium or a combination of the two, the heating rate is 1 to 10°C / min, the carbonization temperature is 1200 to 1700°C (1400 to 1500°C according to a preferred implementation manner), and the carbonization time is 1 to 4h.

[0054] The prepared coal-based carbon material is an amorphous hard carbon material.

[0055] The above method can be used to prepare a coal-based carbon material, wherein the interlayer spacing of the coal-based carbon material is 0.377 to 0.383 nm.

[0056] The prepared coal-based carbon material can be used as a negative electrode material for sodium ion batteries to prepare negative electrodes for sodium ion batteries. The negative electrode material can be placed on the surface of a negative electrode current collector to prepare a negative electrode. The common methods in the art can be used, such as coating the provided negative electrode material for sodium ion batteries on a current collector to form the negative electrode. The current collector used can be a conventional material in the art. Furthermore, the negative electrode and positive electrode, a separator and an electrolyte can be assembled into a sodium ion secondary battery.

[0057] The protection scheme of the present invention is described below by specific examples. It should be noted that these examples are only used to facilitate the understanding of those skilled in the art and should not be regarded as limiting the scope of protection of the present invention. Unless otherwise specified, the reagents used in the examples can be obtained commercially.

[0058] Example 1

[0059] Example 1 provides a coal-based carbon material for a negative electrode of a sodium ion battery, which is prepared by the following method:

[0060] (1) Take 5 g of bituminous coal and grind it into powder. Soak the powdered bituminous coal in a mixed acid solution of hydrochloric acid and hydrofluoric acid in a volume ratio of 1:1 for 24 hours. Rinse the acid-treated bituminous coal powder with deionized water until it is neutral, and dry the powder.

[0061] (2) 0.5 g of theabrownin was mixed with the dry coal powder obtained in step (1), and then pre-oxidized at 300° C. for 9 h in an air atmosphere.

[0062] (3) The pre-oxidation product obtained in step (2) is placed in a tubular furnace, and the temperature is increased to 1400° C. at a rate of 5° C. / min under an argon atmosphere, and the temperature is maintained constant for 2 hours to prepare a coal-based carbon sodium ion battery negative electrode material.

[0063] After characterization, the prepared coal-based carbon layer spacing is 0.383nm. As the negative electrode of sodium ion battery, the first discharge specific capacity is 439.78mAh / g at a current density of 0.1A / g.-1 , the first coulombic efficiency is 75.8%.

[0064] Example 2

[0065] Example 2 provides a coal-based carbon material for a negative electrode of a sodium ion battery, which is prepared by the following method:

[0066] (1) 5 g of bituminous coal was crushed and soaked in a mixed acid solution of hydrochloric acid and hydrofluoric acid in a volume ratio of 2:1 for 12 h. The acid-treated bituminous coal powder was rinsed with deionized water until it was neutral, and the powder was dried;

[0067] (2) mixing 1.5 g of theabrownin with the dry coal powder obtained in step (1), and then pre-oxidizing at 330° C. for 6 h in an oxygen atmosphere;

[0068] (3) The pre-oxidation product obtained in step (2) is placed in a tubular furnace, and the temperature is increased to 1300° C. at a rate of 6° C. / min under a nitrogen atmosphere, and the temperature is maintained constant for 3 hours to prepare a coal-based carbon sodium ion battery negative electrode material.

[0069] After characterization, the prepared coal-based carbon layer spacing is 0.379nm. As the negative electrode of the sodium ion battery, the first discharge capacity is 420mAh / g at a current density of 0.1A / g. -1 , the first coulombic efficiency is 74%.

[0070] Example 3

[0071] Example 3 provides a coal-based carbon material for a negative electrode of a sodium ion battery, which is prepared by the following method:

[0072] (1) 4 g of bituminous coal was crushed and soaked in a mixed acid solution of hydrochloric acid and hydrofluoric acid in a volume ratio of 3:1 for 18 h. The acid-treated bituminous coal powder was rinsed with deionized water until it was neutral, and the powder was dried;

[0073] (2) mixing 1.2 g of theabrownin with the dry coal powder obtained in step (1), and then pre-oxidizing at 270° C. for 12 h in an oxygen atmosphere;

[0074] (3) The pre-oxidation product obtained in step (2) is placed in a tubular furnace, and the temperature is increased to 1500° C. at a rate of 3° C. / min under an argon atmosphere, and the temperature is maintained constant for 1 hour to prepare a coal-based carbon sodium ion battery negative electrode material.

[0075] After characterization, the prepared coal-based carbon layer spacing is 0.377nm. As the negative electrode of sodium ion battery, the first discharge specific capacity is 497mAh / g at a current density of 0.1A / g. -1 , the first coulombic efficiency is 78%.

[0076] Example 4

[0077] Example 4 provides a coal-based carbon material for a negative electrode of a sodium ion battery, which is prepared by the following method:

[0078] (1) 5 g of bituminous coal was crushed and soaked in a mixed acid solution of hydrochloric acid and hydrofluoric acid in a volume ratio of 1:1 for 12 h. The acid-treated bituminous coal powder was rinsed with deionized water until it was neutral, and the powder was dried;

[0079] (2) mixing 2.0 g of theabrownin with the dry coal powder obtained in step (1), and then pre-oxidizing at 325° C. for 7 h in an air atmosphere;

[0080] (3) The pre-oxidation product obtained in step (2) is placed in a tubular furnace, and the temperature is increased to 1500° C. at a rate of 4° C. / min under a nitrogen atmosphere, and the temperature is maintained constant for 1 hour to prepare a coal-based carbon sodium ion battery negative electrode material.

[0081] The interlayer spacing of the prepared coal-based carbon was characterized to be 0.381nm. As the negative electrode of the sodium ion battery, the first discharge capacity was 444mAh / g at a current density of 0.1A / g. -1 , the first coulombic efficiency is 75%.

[0082] Comparative Example 1

[0083] Comparative Example 1 provides a coal-based carbon material for a negative electrode of a sodium ion battery, which is prepared by the following method:

[0084] (1) 5 g of bituminous coal was crushed and soaked in a mixed acid solution of hydrochloric acid and hydrofluoric acid in a volume ratio of 1:1 for 24 h. The acid-treated bituminous coal powder was rinsed with deionized water until it was neutral, and the powder was dried;

[0085] (2) The above-mentioned coal powder was heated to 1400°C at a rate of 5°C / min under an argon atmosphere and kept at a constant temperature for 2 hours to prepare a coal-based carbon sodium ion battery negative electrode material.

[0086] After characterization, the prepared coal-based carbon layer spacing is 0.368nm. As the negative electrode of sodium ion battery, the first discharge capacity is 340mAh / g at a current density of 0.1A / g. -1 , the first coulombic efficiency is 63%.

[0087] Comparative Example 2

[0088] Comparative Example 2 provides a coal-based carbon material for a negative electrode of a sodium ion battery, which is prepared by the following method:

[0089] (1) 5 g of bituminous coal was crushed and soaked in a mixed acid solution of hydrochloric acid and hydrofluoric acid in a volume ratio of 1:1 for 24 h. The acid-treated bituminous coal powder was rinsed with deionized water until it was neutral, and the powder was dried;

[0090] (2) pre-oxidizing the dry coal powder obtained in step (1) at 300° C. for 9 h in an air atmosphere;

[0091] (3) The pre-oxidation product obtained in step (2) is heated to 1400° C. at a rate of 5° C. / min under an argon atmosphere and kept at a constant temperature for 2 hours to prepare a coal-based carbon sodium ion battery negative electrode material.

[0092] After characterization, the prepared coal-based carbon layer spacing is 0.373nm. As the negative electrode of sodium ion battery, the first discharge specific capacity is 419mAh / g at a current density of 0.1A / g. -1 , the first coulombic efficiency is 68%.

[0093] It is not difficult to see from the above embodiments and comparative examples that the method provided by the present invention can improve coal-based carbon materials with poor sodium storage performance, and further improve the reversible specific capacity and first-cycle coulombic efficiency of coal-based carbon materials.

[0094] The applicant declares that the present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0095] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "specific implementation methods", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.

[0096] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a coal-based carbon negative electrode material for a sodium ion battery, It is characterized in that include: (1) soaking the bituminous coal in a mixed acid solution containing hydrochloric acid and hydrofluoric acid, rinsing until the solution is neutral, and then drying to obtain dry coal powder; (2) mixing the theabrownin with the dry coal powder obtained in step (1), and performing a pre-oxidation treatment in an oxygen-containing atmosphere to obtain a pre-oxidation product; (3) Carbonizing the pre-oxidation product under an inert atmosphere to obtain a coal-based carbon material.

2. The preparation method according to claim 1, It is characterized in that The bituminous coal in step (1) is pre-crushed, and the particle size of the crushed bituminous coal is 45 microns to 74 microns.

3. The preparation method according to claim 1, It is characterized in that The volume ratio of hydrochloric acid to hydrofluoric acid in the mixed acid solution containing hydrochloric acid and hydrofluoric acid in step (1) is (1-4):(1-4); Optionally, the soaking treatment time in step (1) is 5 to 48 hours.

4. The preparation method according to claim 1, It is characterized in that The mass ratio of theabrownin to dry coal powder in step (2) is (1-6):(1-6).

5. The preparation method according to claim 1, It is characterized in that The oxygen-containing atmosphere in step (2) is selected from at least one of air, oxygen and ozone; Optionally, the inert atmosphere in step (3) is at least one of argon, nitrogen and helium.

6. The preparation method according to claim 1, It is characterized in that The temperature of the pre-oxidation treatment in step (2) is 200-400° C. Optionally, the pre-oxidation treatment time in step (2) is 1-12 hours.

7. The preparation method according to claim 1, It is characterized in that The carbonization temperature in step (3) is 1200-1700° C. Optionally, the carbonization time in step (3) is 1 to 4 hours; Optionally, the heating rate of the carbonization in step (3) is 1 to 10°C / min.

8. A coal-based carbon negative electrode material for sodium ion batteries, It is characterized in that It is prepared by the preparation method described in any one of claims 1 to 7.

9. A sodium ion battery negative electrode, It is characterized in that Including the coal-based carbon negative electrode material for sodium ion battery as described in claim 8.

10. A sodium ion battery, It is characterized in that Including the sodium ion battery negative electrode as described in claim 9.

Citation Information

Patent Citations

  • Rough extraction method and fine extraction method of theabrownine

    CN104082452A

  • Method for manufacturing carbon molecular sieves by using oil tea shells

    CN107321307A

  • Direction control method of surface oxygen functional groups on coal-based hard carbon for sodium-storing cathodes

    CN109796003A

  • Activated carbon and preparation method thereof

    CN112573519A

  • Cobalt oxide-hydroxylated single-walled carbon nanotube composite material and preparation and application thereof

    CN113003614A

Cited By

  • Method for preparing coal-based hard carbon material by oxygen-assisted low-temperature etching of amorphous components in coal precursor

    CN119976792A

  • Method and device for preparing hard carbon negative electrode material based on lignite

    CN121452824A