Carbon nano tube based on metal organic framework material as well as low-temperature synthesis method and application of carbon nano tube

Through the low-temperature synthesis method based on metal-organic framework materials, the problems of high-temperature synthesis of carbon nanotubes and harsh catalyst preparation are solved, the simplicity and efficiency of the low-temperature process are achieved, and the scope of its application is expanded.

CN118754109APending Publication Date: 2024-10-11TONGJI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411031128.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing carbon nanotube synthesis methods require high-temperature conditions and harsh catalyst preparation conditions, and the low-temperature synthesis method of carbon nanotubes has not yet been effectively solved, limiting their wide application.

Method used

A low-temperature synthesis method based on metal-organic framework materials is used. The methanol solution of cobalt nitrate hexahydrate and 2-methylimidazole is mixed to form a metal-organic framework material precursor liquid. After being coated on the substrate, temperature-raising pyrolysis and low-temperature chemical vapor deposition are performed to achieve carbonization. Low temperature synthesis of nanotubes.

Benefits of technology

Achieved low-temperature synthesis of carbon nanotubes with simple process and low energy consumption, reduced energy consumption and cost, expanded the synthesis and application of carbon nanotubes, shortened the annealing time, and improved the accessibility of cobalt atoms and carbon The length of the nanotube.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754109A_ABST
    Figure CN118754109A_ABST
Patent Text Reader

Abstract

The invention relates to a carbon nanotube based on a metal organic framework material and a low-temperature synthesis method and application thereof, and the synthesis method comprises the following specific steps: S1, mixing a methanol solution of cobalt nitrate hexahydrate and a methanol solution of 2-methylimidazole to obtain a precursor solution of the metal organic framework material; s2, coating a substrate with the precursor solution of the metal organic framework material obtained in the step S1 to obtain the substrate with a metal organic framework growing on the surface; and S3, sequentially carrying out heating pyrolysis and low-temperature chemical vapor deposition on the substrate with the metal organic framework growing on the surface obtained in the step S2 to obtain the carbon nanotube. Compared with the prior art, the metal organic framework material which is simple in process and low in cost is adopted as the precursor of the catalyst for growing the carbon nanotubes, a traditional evaporation coating method which is high in energy consumption and complex in process does not need to be adopted, and the pyrolysis temperature of the metal organic framework and the growth temperature of the carbon nanotubes are low; and the carbon nanotube can be grown on a common material substrate at low temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of carbon nanotube synthesis, and in particular to a carbon nanotube based on a metal organic framework material and a low-temperature synthesis method and application thereof. Background Art

[0002] The unique structure of carbon nanotubes (CNTs) gives them excellent mechanical, electrochemical, electrical and thermal properties, and they have important application value and prospects in many fields such as integrated circuits, catalysis, energy conversion and storage, and flexible wearable electronic devices.

[0003] At present, the synthesis methods of carbon nanotubes mainly include arc discharge method, laser ablation method, combustion method, chemical vapor deposition method (CVD), etc., all of which need to be carried out under high temperature conditions. The low-temperature synthesis method of carbon nanotubes still has great challenges. For the CVD method, low-temperature synthesis of carbon nanotubes can be achieved through the careful design of metal catalysts and the use of plasma or microwave-assisted technologies, but the preparation conditions of the catalyst are still relatively harsh and the synthesis process also requires special equipment, which to a certain extent limits the synthesis and wide application of carbon nanotubes.

[0004] In recent years, metal organic frameworks (such as zeolite imidazolate frameworks, ZIFs) with highly uniform metal atoms in their molecular structures can be used to synthesize carbon nanotubes through high-temperature pyrolysis or vapor deposition processes, but the following problems still exist: 1) The pyrolysis temperature is high, usually 600-1000°C, and the time is long (6h); 2) Catalyst particles are easy to aggregate, making it difficult to achieve continuous growth of carbon nanotubes.

[0005] Chinese patent CN201710128763.8 discloses a method for preparing a nanostructure assembled by carbon nanotubes at low temperature based on metal organic framework compounds, comprising the following steps: S1, weighing appropriate amounts of metal salts and organic ligands respectively, and through liquid phase synthesis, the metal ions and organic ligands in the solvent undergo coordination reaction to form metal organic framework compounds, and washing to obtain metal organic framework compound powder; S2, placing the powder obtained in step S1 in an oven at 80-100°C for 5-10 hours; S3, slowly heating and keeping the metal organic framework compound powder obtained in step S2 in an inert atmosphere to obtain a nanostructure material assembled by carbon nanotubes. In the subsequent preparation of electrodes in the patent, inactive substances such as PVDF binders are also required, which reduces the energy density of the battery (Example 1

[0048] ); and the annealing process in the patent (roughly calculating the heating and holding time) is at least 11 hours.

[0006] Therefore, it is of great theoretical and practical significance to realize the low-temperature synthesis of CNTs by utilizing the highly uniformly distributed metal atoms in metal-organic framework materials. Summary of the invention

[0007] The purpose of the present invention is to provide a carbon nanotube based on a metal organic framework material and a low-temperature synthesis method and application thereof. The carbon nanotube synthesis method has a simple process and low energy consumption.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] A low-temperature synthesis method of carbon nanotubes based on metal organic framework materials, the specific steps are as follows:

[0010] S1, mixing a methanol solution of cobalt nitrate hexahydrate and a methanol solution of 2-methylimidazole to obtain a precursor solution of a metal organic framework material;

[0011] S2, coating the precursor solution of the metal organic framework material obtained in step S1 on the substrate to obtain a substrate with a metal organic framework grown on the surface;

[0012] S3, subjecting the substrate with the surface-grown metal organic framework obtained in step S2 to temperature-increasing pyrolysis and low-temperature chemical vapor deposition in sequence to obtain carbon nanotubes.

[0013] Furthermore, in step S1, the metal organic framework material is ZIF-67.

[0014] Furthermore, in step S1, the concentration of the methanol solution of cobalt nitrate hexahydrate is 0.1 to 0.6 mol / L;

[0015] The concentration of the 2-methylimidazole methanol solution is 1.0-2.0 mol / L.

[0016] Furthermore, in step S1, the molar ratio of the cobalt nitrate hexahydrate to 2-methylimidazole is 1:(4-8).

[0017] Furthermore, in step S1, the mixing and stirring temperature is room temperature, the mixing and stirring speed is 200 to 1000 rpm, and the mixing and stirring time is 10 to 60 min.

[0018] Furthermore, in step S2, the substrate includes a conductive substrate and a non-conductive substrate, and the specific preparation method of the substrate with the metal organic framework grown on the surface is as follows:

[0019] When the substrate is a conductive substrate: electrodepositing cobalt hydroxide nanosheets on the conductive substrate, and then immersing the conductive substrate in the precursor solution of the metal organic framework material obtained in step S1, and growing a metal organic framework layer on the surface of the substrate after reacting for a certain period of time at room temperature and pressure, to obtain a substrate with a metal organic framework grown on the surface;

[0020] When the substrate is a non-conductive substrate: the precursor liquid of the metal organic framework material obtained in step S1 is dropwise coated on the surface of the non-conductive substrate, dried, and then immersed in the precursor liquid of the metal organic framework material obtained in step S1, and a metal organic framework layer is grown on the surface of the substrate after reacting for a certain period of time at room temperature and pressure to obtain a substrate with a metal organic framework grown on the surface.

[0021] Furthermore, in the above, the conductive substrate includes stainless steel foil, titanium foil, aluminum foil, copper foil, stainless steel mesh, titanium mesh, copper foam, etc.

[0022] Furthermore, in the above, the non-conductive substrate is glass.

[0023] Furthermore, the specific conditions for electrodepositing cobalt hydroxide nanosheets on the conductive substrate are as follows:

[0024] A cobalt nitrate aqueous solution with a concentration of 0.1 to 0.6 mol / L is prepared as an electrodeposition electrolyte, a conductive substrate is used as a working electrode, a platinum sheet is used as a counter electrode, Ag / AgCl is used as a reference electrode, a deposition voltage is -1.5 to -0.5 V, and a deposition time is 100 to 1000 s.

[0025] Furthermore, in the above, the reaction time at normal temperature and pressure is 1 to 12 hours.

[0026] Furthermore, in step S3, the specific preparation method of the carbon nanotubes is as follows:

[0027] The substrate with the surface-grown metal organic framework obtained in step S2 is placed in a tubular furnace and heated under the protection of an inert gas. As the metal organic framework is pyrolyzed, the cobalt atoms therein aggregate in situ to form nanoparticles. Hydrogen and carbon source gas are continuously introduced at high temperature to perform chemical vapor deposition in situ growth to obtain carbon nanotubes.

[0028] Furthermore, in the above, the tube furnace is heated from room temperature to 400°C to 600°C, preferably to 500°C, under the protection of the inert gas.

[0029] In the above, the inert gas is argon, the flow rate is 40 to 120 sccm, and the heating rate is 10 to 25°C / min;

[0030] The flow rate of high-temperature hydrogen is 10-60 sccm, the flow rate of carbon source gas is 2-50 sccm, and the in-situ growth time is 5-120 minutes.

[0031] In the above further aspect, the carbon source gas is ethylene.

[0032] The present invention also provides a carbon nanotube based on a metal organic framework material, wherein the carbon nanotube is obtained by the above-mentioned low-temperature synthesis method.

[0033] Furthermore, the carbon nanotubes grow densely and are curved in shape, and multiple carbon nanotubes are intertwined with each other. The diameter of a single carbon nanotube is 10 to 20 nm, and the length of a single carbon nanotube is 1 to 2 μm.

[0034] Furthermore, the carbon nanotubes present an obvious multi-wall structure, with an outer diameter of 10 to 20 nm and an inner diameter of 3 to 5 nm.

[0035] In the above, further, the top of the multi-walled carbon nanotube is encapsulated with cobalt nanoparticles, and the diameter of the cobalt nanoparticles is 8-12 nm.

[0036] Furthermore, the carbon nanotubes have a multi-level pore size distribution, with micropores and mesopores coexisting.

[0037] In addition, the present invention also provides an application of carbon nanotubes based on metal organic framework materials, wherein the carbon nanotubes are used to prepare flexible wearable electronic devices.

[0038] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0039] 1. The present invention uses a metal organic framework material with simple process and low cost as a precursor for growing carbon nanotube catalysts, without the need to use the traditional evaporation coating method with high energy consumption and complex process, which can significantly reduce energy consumption and cost.

[0040] 2. The pyrolysis temperature of the metal organic framework and the growth temperature of carbon nanotubes of the present invention are low (about 500°C), and carbon nanotubes can be grown at low temperature on common material substrates (such as ordinary glass, etc.), which can effectively expand the synthesis and application of carbon nanotubes.

[0041] 3. In the low-temperature synthesis method of carbon nanotubes based on the metal organic framework material ZIF-67 of the present invention, a simple solution method is used to synthesize ZIF-67 as a catalyst precursor for growing carbon nanotubes. Compared with the traditional evaporation coating method with high energy consumption and complex process, the process of the present invention is simpler and more efficient;

[0042] 4. In the low-temperature synthesis method of carbon nanotubes based on the metal organic framework material ZIF-67 of the present invention, compared with the traditional CVD method for synthesizing carbon nanotubes, the synthesis temperature is low; compared with other methods for synthesizing carbon nanotubes using metal organic framework materials, the time is shorter, the process is efficient and the energy consumption is low.

[0043] 5. The low-temperature synthesis method of carbon nanotubes based on the metal organic framework material ZIF-67 of the present invention can realize the low-temperature synthesis of carbon nanotubes on a variety of conventional substrates, thereby effectively expanding the practical application of carbon nanotube materials.

[0044] 6. The present invention innovates the pre-treatment method: the combination of ZIF-67 and a variety of substrates can be achieved through the process of electrodeposition + in-situ growth, and the modification of the substrate can be directly achieved through the subsequent chemical vapor deposition (CVD) growth process, breaking through the limitation of powder. In subsequent applications, the modified (growing carbon nanotubes) substrate can be directly used as a self-supporting electrode.

[0045] 7. The present invention innovates the annealing conditions: during the low-temperature pyrolysis process of rapidly heating to 500°C, the originally polyhedral ZIF-67 crystals are broken and cobalt nanoparticles are formed, thereby forming carbon nanosheets loaded with cobalt nanoparticles, which provide a good platform for the subsequent growth of CNTs by CVD method; compared with the existing patents, the present invention greatly shortens the time of the annealing process. The method of the present invention only takes 2.4 hours at most, and 30 minutes at least.

[0046] 8. Unlike existing patents that retain the polyhedral framework of ZIF (only the cobalt atoms on the surface can be used), the method of the present invention causes the ZIF framework to break to form carbon nanosheets, thereby increasing the accessibility of cobalt atoms. The internal cobalt atoms can also be used, thereby forming more cobalt catalyst particles.

[0047] 9. The existing patent only uses ZIF itself as a carbon source. The length of the carbon nanotubes in this method is 200-500nm. However, the present invention introduces an external carbon source C under the condition of 500℃ insulation. 2 H 4 There is no problem of insufficient carbon source, and the obtained carbon nanotubes are longer, with a length of 1 to 2 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 The figure is a schematic flow chart of the low-temperature synthesis method of carbon nanotubes based on metal organic framework material (ZIF-67) of the present invention.

[0049] Figure 2 These are low-magnification scanning electron microscope images and optical photographs of the metal organic framework ZIF-67@stainless steel foil substrate prepared in Example 1.

[0050] Figure 3 This is a high-magnification scanning electron microscope image of the metal organic framework ZIF-67@stainless steel foil substrate prepared in Example 1.

[0051] Figure 4 This is a low-magnification scanning electron microscope image of the carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67 prepared in Example 1.

[0052] Figure 5This is a high-magnification scanning electron microscope image of the carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67 prepared in Example 1.

[0053] Figure 6 This is a low-magnification transmission electron microscope image of the carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67 prepared in Example 1.

[0054] Figure 7 This is a high-magnification transmission electron microscope image of the carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67 prepared in Example 1.

[0055] Figure 8 This is the X-ray diffraction pattern of the carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67 prepared in Example 1.

[0056] Fig. 9 This is the Raman spectrum of the carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67 prepared in Example 1.

[0057] Fig.10 This is the nitrogen adsorption-desorption isotherm diagram of the carbon nanotubes based on the metal organic framework ZIF-67 prepared in Example 1.

[0058] Fig.11 This is the pore size distribution diagram of the carbon nanotubes based on the metal organic framework ZIF-67 prepared in Example 1.

[0059] Fig.12 This is an optical photograph of the metal organic framework ZIF-67@copper foam substrate prepared in Example 2.

[0060] Fig.13 This is a scanning electron microscope image of the metal organic framework ZIF-67@copper foam substrate prepared in Example 2.

[0061] Fig.14 This is an optical photograph of the carbon nanotube@copper foam substrate based on the metal organic framework ZIF-67 prepared in Example 2.

[0062] Fig.15 This is a scanning electron microscope image of the carbon nanotube@copper foam substrate based on the metal organic framework ZIF-67 prepared in Example 2.

[0063] Fig.16 This is an optical photograph of the metal organic framework ZIF-67@glass substrate prepared in Example 3.

[0064] Fig.17 This is a scanning electron microscope image of the metal organic framework ZIF-67@glass substrate prepared in Example 3.

[0065] Fig.18 This is an optical photograph of the carbon nanotubes@glass substrate based on the metal organic framework ZIF-67 prepared in Example 3.

[0066] Fig.19 This is a scanning electron microscope image of the carbon nanotubes@glass substrate based on the metal organic framework ZIF-67 prepared in Example 3.

[0067] Fig. 20 Schematic diagram of the change in conductivity of the glass surface in ordinary soda-lime glass and carbon nanotube@glass substrate based on metal organic framework ZIF-67 prepared in Example 3, wherein a) is ordinary soda-lime glass, and b) is glass after carbon nanotube growth.

[0068] Fig.21 SEM image of carbon nanosheets loaded with cobalt nanoparticles.

[0069] Fig. 22 TEM image of carbon nanosheets loaded with cobalt nanoparticles.

[0070] Fig.23 This is a high-magnification transmission electron microscope image of a single carbon nanotube based on the metal organic framework ZIF-67 prepared in Example 1 on a stainless steel foil substrate. DETAILED DESCRIPTION

[0071] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0072] In conjunction with the accompanying drawings, some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.

[0073] Embodiment 1:

[0074] This embodiment provides a low-temperature synthesis method of carbon nanotubes based on metal organic framework materials. The carbon nanotubes are synthesized at low temperature on a stainless steel foil substrate. The schematic diagram of the preparation process is shown in FIG. Figure 1 As shown, the specific steps are as follows:

[0075] (1) mixing 10 mL of a 0.2 mol / L methanol solution of cobalt nitrate hexahydrate and 10 mL of a 1.6 mol / L methanol solution of 2-methylimidazole at 500 rpm for 30 min to obtain a precursor solution for synthesizing a metal organic framework material (ZIF-67);

[0076] (2) Prepare 80 mL of 0.1 mol / L cobalt nitrate aqueous solution as the electrodeposition electrolyte, take a piece of stainless steel foil (length and width are 1 cm) as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl as the reference electrode, and electrodeposit cobalt hydroxide on the stainless steel foil at a constant voltage of -1.0 V for 400 s.

[0077] (3) Immersing the cobalt hydroxide loaded stainless steel foil obtained in step (2) into the ZIF-67 precursor solution in step (1) to obtain a ZIF-67@stainless steel foil substrate material.

[0078] (4) The ZIF-67@stainless steel foil substrate material obtained in step (3) is placed in a tube furnace, and the tube furnace is heated from room temperature to 500° C. at a heating rate of 20° C. / min in argon with a flow rate of 80 sccm, and then 20 sccm of hydrogen and 5 sccm of ethylene are introduced at 500° C. to perform chemical vapor deposition to grow carbon nanotubes for a growth time of 120 min, thereby obtaining carbon nanotubes based on the metal organic framework ZIF-67 supported on the stainless steel foil, i.e., carbon nanotubes@stainless steel foil substrate.

[0079] The specific test results of this embodiment are as follows:

[0080] Figure 2 and Figure 3 This is a scanning electron microscope photo of the prepared metal organic framework ZIF-67. Figure 2 The illustration in the upper right corner is an optical image of the ZIF-67@stainless steel foil substrate. It can be seen that the ZIF-67 nanoparticles have no obvious vacancies on the stainless steel foil surface and the particle morphology is uniform. A single nanoparticle is a polyhedron with a size of about 500 nm.

[0081] Figure 4 and Figure 5 This is a scanning electron microscope image of the prepared carbon nanotubes @ stainless steel foil substrate based on the metal organic framework ZIF-67. From the image, it can be seen that the carbon nanotubes @ stainless steel foil substrate based on the metal organic framework ZIF-67 grow densely, are curved, and are intertwined with each other. The diameter of a single carbon nanotube is about 10 to 20 nm.

[0082] Fig.23 This is a high-magnification transmission electron microscope image of a single carbon nanotube based on the metal organic framework ZIF-67 prepared in Example 1 on a stainless steel foil substrate. The length of the carbon tube is 1 to 2 μm.

[0083] Figure 6 and Figure 7This is the transmission electron microscope image of the prepared carbon nanotubes @ stainless steel foil substrate based on the metal organic framework ZIF-67. It can be seen that the carbon nanotubes @ stainless steel foil substrate grown at low temperature based on the metal organic framework ZIF-67 presents an obvious multi-walled structure with an outer diameter of about 10 to 20 nm and an inner diameter of about 3 to 5 nm. Cobalt nanoparticles with a diameter of about 10 nm are encapsulated at the top of the multi-walled carbon nanotubes.

[0084] Figure 8 The X-ray diffraction pattern of the prepared carbon nanotubes @ stainless steel foil substrate based on the metal organic framework ZIF-67 is shown in the figure, showing the typical carbon nanotube (002) diffraction peak of the carbon nanotubes @ stainless steel foil substrate based on the metal organic framework ZIF-67 and the (111) diffraction peak of the cobalt nanoparticles.

[0085] Fig. 9 This is the Raman spectrum of the prepared carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67. The characteristic peak of the carbon nanotubes@stainless steel foil substrate appears at 1350 cm -1 and 1590cm -1 , corresponding to the D peak and the G peak respectively.

[0086] Fig.10 The nitrogen adsorption-desorption isotherm of the prepared carbon nanotubes@stainless steel foil substrate based on the metal organic framework ZIF-67. The BET specific surface area is calculated to be 118 cm 2 / g, showing that the prepared carbon nanotubes based on metal organic framework ZIF-67@stainless steel foil substrate has a large specific surface area. The adsorption-desorption curve in the figure shows an obvious combination of type I and type IV isotherms, indicating the multi-level pore size distribution structure of the prepared carbon nanotubes based on metal organic framework ZIF-67@stainless steel foil substrate.

[0087] Fig.11 The pore size distribution diagram of the prepared carbon nanotubes @ stainless steel foil substrate based on metal organic framework ZIF-67 shows that the prepared carbon nanotubes @ stainless steel foil substrate based on metal organic framework ZIF-67 has a structure in which micropores and mesopores coexist.

[0088] Example 2

[0089] This embodiment provides a low-temperature synthesis method of carbon nanotubes based on metal organic framework materials. The carbon nanotubes are synthesized at low temperature on a copper foam substrate. The schematic diagram of the preparation process is shown in FIG. Figure 1 As shown, the specific steps are as follows:

[0090] (1) mixing 10 mL of a 0.2 mol / L methanol solution of cobalt nitrate hexahydrate and 10 mL of a 1.6 mol / L methanol solution of 2-methylimidazole at 500 rpm for 30 min to obtain a precursor solution for synthesizing a metal organic framework material (ZIF-67);

[0091] (2) Prepare 80 mL of 0.1 mol / L cobalt nitrate aqueous solution as the electrodeposition electrolyte, take a piece of copper foam (length and width are 1 cm) as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl as the reference electrode, and electrodeposit cobalt hydroxide on the copper foam at a constant voltage of -1.5 V for 300 s.

[0092] (3) Immersing the copper foam loaded with cobalt hydroxide obtained in step (2) into the precursor solution of ZIF-67 in step (1) to obtain a ZIF-67@copper foam substrate material.

[0093] (4) The ZIF-67@copper foam substrate material obtained in step (3) is placed in a tube furnace, and the tube furnace is heated from room temperature to 500° C. at a heating rate of 20° C. / min in an argon gas with a flow rate of 80 sccm, and then 20 sccm of hydrogen and 3 sccm of ethylene are introduced at 500° C. to perform chemical vapor deposition to grow carbon nanotubes for a growth time of 60 min, thereby obtaining carbon nanotubes based on the metal organic framework ZIF-67 supported on copper foam, i.e., carbon nanotubes@copper foam substrate.

[0094] The specific test results of this embodiment are as follows:

[0095] Fig.12 This is an optical photograph of the prepared metal organic framework ZIF-67@copper foam substrate. From the picture, we can see that the ZIF-67 nanoparticles are well loaded on the copper foam and there are no obvious vacancies on the substrate.

[0096] Fig.13 This is a scanning electron microscope image of the prepared metal organic framework ZIF-67@copper foam substrate. It can be seen from the image that ZIF-67 nanoparticles are evenly loaded on the copper foam.

[0097] Fig.14 This is an optical photograph of the prepared carbon nanotubes@copper foam substrate based on the metal organic framework ZIF-67. From the picture, it can be seen that the carbon nanotubes based on the metal organic framework ZIF-67 are successfully grown on the copper foam.

[0098] Fig.15This is a scanning electron microscope image of the prepared carbon nanotubes@copper foam substrate based on the metal organic framework ZIF-67. From the image, it can be seen that the carbon nanotubes based on the metal organic framework ZIF-67 grow evenly on the copper foam skeleton and are in a curved and entangled state.

[0099] Example 3

[0100] This embodiment provides a low-temperature synthesis method of carbon nanotubes based on metal organic framework materials. The carbon nanotubes are synthesized at low temperature on a glass substrate. The preparation process is shown in the schematic diagram. Figure 1 As shown, the specific steps are as follows:

[0101] (1) mixing 10 mL of a 0.2 mol / L methanol solution of cobalt nitrate hexahydrate and 10 mL of a 1.6 mol / L methanol solution of 2-methylimidazole at 500 rpm for 30 min to obtain a precursor solution for synthesizing a metal organic framework material (ZIF-67);

[0102] (2) The precursor solution obtained in step (1) is evenly dropped onto the glass surface, dried in a vacuum oven at 60° C., and then immersed in the precursor solution of ZIF-67 in step (1) to obtain a ZIF-67@glass substrate material.

[0103] (4) The ZIF-67@glass substrate material obtained in step (3) is placed in a tube furnace, and the tube furnace is heated from room temperature to 500°C at a heating rate of 20°C / min in argon with a flow rate of 80sccm, and then 30sccm of hydrogen and 5sccm of ethylene are introduced at 500°C to perform chemical vapor deposition to grow carbon nanotubes for a growth time of 120min, thereby obtaining carbon nanotubes based on the metal organic framework ZIF-67 supported on glass, i.e., carbon nanotubes@glass substrate.

[0104] Fig.16 This is an optical photograph of the prepared metal-organic framework ZIF-67@glass substrate. From the picture, we can see that the ZIF-67 nanoparticles are well loaded on the glass surface and there are no obvious vacancies on the substrate.

[0105] Fig.17 This is a scanning electron microscope image of the prepared metal organic framework ZIF-67@glass substrate. It can be seen from the image that ZIF-67 nanoparticles are evenly loaded on the glass surface.

[0106] Fig.18 This is an optical photograph of the prepared carbon nanotubes based on the metal organic framework ZIF-67@glass substrate. From the picture, it can be seen that the carbon nanotubes based on the metal organic framework ZIF-67 grow on glass.

[0107] Fig.19This is a scanning electron microscope image of the prepared carbon nanotubes based on the metal organic framework ZIF-67@glass substrate. From the image, it can be seen that the carbon nanotubes based on the metal organic framework ZIF-67 grow in large quantities on the glass surface, appearing in a curved and entangled state.

[0108] Fig. 20 Schematic diagram of the change in surface conductivity of glass in ordinary soda-lime glass and carbon nanotubes@glass substrate based on metal organic framework ZIF-67 prepared in Example 3, wherein the surface of ordinary soda-lime glass is insulating, and the conductivity of the glass is improved after the growth of carbon nanotubes.

[0109] Example 4

[0110] This embodiment provides a method for preparing a carbon nanosheet loaded with cobalt nanoparticles, and the specific steps are as follows:

[0111] (1) mixing 10 mL of a 0.2 mol / L methanol solution of cobalt nitrate hexahydrate and 10 mL of a 1.6 mol / L methanol solution of 2-methylimidazole at 500 rpm for 30 min to obtain a precursor solution for synthesizing a metal organic framework material (ZIF-67);

[0112] (2) The precursor solution obtained in step (1) is evenly dropped onto the glass surface, dried in a vacuum oven at 60° C., and then immersed in the precursor solution of ZIF-67 in step (1) to obtain a ZIF-67@glass substrate material.

[0113] (4) The ZIF-67@glass substrate material obtained in step (3) is placed in a tube furnace, and the tube furnace is heated from room temperature to 500° C. at a heating rate of 20° C. / min in an argon gas with a flow rate of 80 sccm to obtain a carbon nanosheet loaded with cobalt nanoparticles.

[0114] like Figures 21-22 As shown, during the low-temperature pyrolysis process of rapidly heating to 500°C, the originally polyhedral ZIF-67 crystals were broken and cobalt nanoparticles were formed at the same time, thereby forming carbon nanosheets loaded with cobalt nanoparticles, providing a good platform for the subsequent growth of CNTs by CVD method.

[0115] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A low-temperature synthesis method of carbon nanotubes based on metal organic framework materials, characterized in that: The specific steps are as follows: S1, mixing a methanol solution of cobalt nitrate hexahydrate and a methanol solution of 2-methylimidazole to obtain a precursor solution of a metal organic framework material; S2, coating the precursor solution of the metal organic framework material obtained in step S1 on the substrate to obtain a substrate with a metal organic framework grown on the surface; S3, subjecting the substrate with the surface-grown metal organic framework obtained in step S2 to temperature-increasing pyrolysis and low-temperature chemical vapor deposition in sequence to obtain carbon nanotubes.

2. The low-temperature synthesis method of carbon nanotubes based on metal organic framework materials according to claim 1, characterized in that: In step S1, the concentration of the methanol solution of cobalt nitrate hexahydrate is 0.1-0.6 mol / L, and the concentration of the methanol solution of 2-methylimidazole is 1.0-2.0 mol / L; The molar ratio of the cobalt nitrate hexahydrate to 2-methylimidazole is 1:(4-8); The mixing and stirring temperature is room temperature, the mixing and stirring speed is 200-1000 rpm, and the mixing and stirring time is 10-60 min.

3. The low-temperature synthesis method of carbon nanotubes based on metal organic framework materials according to claim 1, characterized in that: In step S2, the substrate includes a conductive substrate and a non-conductive substrate, and the specific preparation method of the substrate with the metal organic framework grown on the surface is as follows: When the substrate is a conductive substrate: electrodepositing cobalt hydroxide nanosheets on the conductive substrate, and then immersing the conductive substrate in the precursor solution of the metal organic framework material obtained in step S1, and growing a metal organic framework layer on the surface of the substrate after reacting for a certain period of time at room temperature and pressure, to obtain a substrate with a metal organic framework grown on the surface; When the substrate is a non-conductive substrate: the precursor liquid of the metal organic framework material obtained in step S1 is dropwise coated on the surface of the non-conductive substrate, dried, and then immersed in the precursor liquid of the metal organic framework material obtained in step S1, and a metal organic framework layer is grown on the surface of the substrate after reacting for a certain period of time at room temperature and pressure to obtain a substrate with a metal organic framework grown on the surface.

4. The low-temperature synthesis method of carbon nanotubes based on metal organic framework materials according to claim 3, characterized in that: The conductive substrate includes stainless steel foil, titanium foil, aluminum foil, copper foil, stainless steel mesh, titanium mesh and copper foam. The non-conductive substrate is glass; The specific conditions for electrodepositing cobalt hydroxide nanosheets on the conductive substrate are as follows: A cobalt nitrate aqueous solution with a concentration of 0.1 to 0.6 mol / L is prepared as an electrodeposition electrolyte, a conductive substrate is used as a working electrode, a platinum sheet is used as a counter electrode, Ag / AgCl is used as a reference electrode, a deposition voltage is -1.5 to -0.5 V, and a deposition time is 100 to 1000 s.

5. The low-temperature synthesis method of carbon nanotubes based on metal organic framework materials according to claim 1, characterized in that: In step S3, the specific preparation method of the carbon nanotubes is as follows: The substrate with the surface-grown metal organic framework obtained in step S2 is placed in a tubular furnace and heated under the protection of an inert gas. As the metal organic framework is pyrolyzed, the cobalt atoms therein aggregate in situ to form nanoparticles. Hydrogen and carbon source gas are continuously introduced at high temperature to perform chemical vapor deposition in situ growth to obtain carbon nanotubes.

6. The low-temperature synthesis method of carbon nanotubes based on metal organic framework materials according to claim 5, characterized in that: The tube furnace is heated from room temperature to 400°C to 600°C under the protection of the inert gas. The inert gas is argon, the flow rate is 40-120 sccm, and the heating rate is 10-25°C / min; The flow rate of high-temperature hydrogen is 10-60 sccm, the flow rate of carbon source gas is 2-50 sccm, and the in-situ growth time is 5-120 min; The carbon source gas is ethylene.

7. A carbon nanotube based on a metal organic framework material, characterized in that: The carbon nanotubes are obtained by the low-temperature synthesis method described in any one of claims 1-6.

8. The carbon nanotube based on metal organic framework material according to claim 7, characterized in that: The carbon nanotubes grow densely and are curved in shape. Multiple carbon nanotubes are intertwined with each other. The diameter of a single carbon nanotube is 10 to 20 nm, and the length of a single carbon nanotube is 1 to 2 μm. The carbon nanotubes have a multi-level pore size distribution.

9. The carbon nanotube based on metal organic framework material according to claim 7, characterized in that: The carbon nanotubes have a multi-wall structure, an outer diameter of 10 to 20 nm, and an inner diameter of 3 to 5 nm; Cobalt nanoparticles are encapsulated at the top of the multi-walled carbon nanotubes, and the diameter of the cobalt nanoparticles is 8-12 nm.

10. An application of carbon nanotubes based on metal organic framework materials, characterized in that: The carbon nanotubes obtained by the low-temperature synthesis method described in any one of claims 1 to 6 are used to prepare flexible wearable electronic devices.

Citation Information

Patent Citations

  • A cobalt hydroxide / ZIF-67 carbon-based catalytic electrode and a preparing method and application thereof

    CN109019783A

  • Fabrication method of carbon nanotube or carbon nanofiber using metal-organic frameworks, and the carbon nanotube or carbon nanofiber thereby

    KR1020120092344A