Graphene aerogel wave-absorbing material with wide absorption frequency band as well as preparation and application of graphene aerogel wave-absorbing material
Through the combination of graphene and poly(propionic anhydride) and vapor reduction thermal cross-linking technology, graphene aerogels with wide frequency bands and good mechanical properties are prepared, which solves the problem of narrow absorption band and mechanical properties of existing graphene aerogels. It solves the problem of poor performance and achieves effective absorption of multi-frequency electromagnetic waves.
Patent Information
- Application Number
- CN202410997838.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
AI Technical Summary
Existing graphene airgel absorbing materials have poor mechanical properties and narrow absorption bands, making them unable to effectively deal with multi-band electromagnetic wave pollution.
An aerogel composed of graphene and poly(propionic anhydride) is used. The poly(propionic anhydride) bridges the graphene nanosheets through physical forces, and is prepared through steam reduction and thermal cross-linking to form a product with good mechanical properties and wide frequency band. Absorbent graphene aerogels.
The multi-band electromagnetic wave absorption of graphene aerogel has been realized, the mechanical compression performance and absorption bandwidth have been improved, and it can adapt to the multi-band electromagnetic wave polluted environment.
Smart Images

Figure CN118754111A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electromagnetic wave absorption, and particularly relates to a graphene aerogel absorbing material with a wide absorption band and a preparation method and application thereof. Background Art
[0002] Nowadays, a large number of electronic devices are flooding people's daily lives. Although they have improved the quality of life, they also force the human body to be in an environment of electromagnetic pollution and electromagnetic interference for a long time, which can lead to visual impairment, calcium loss, leukemia and other diseases. In order to solve the problems of electromagnetic pollution and electromagnetic interference, a large number of scientific researchers are committed to the research and development of high-performance absorbing materials.
[0003] Among many high-performance absorbing materials, graphene aerogel not only has the advantages of light weight, large specific surface area, high conductivity, high thermal stability, high chemical stability, etc., but also its abundant pores can enhance the impedance matching between the material and the free space on the one hand, and on the other hand, it can extend the transmission path of electromagnetic waves, thereby enhancing the attenuation of electromagnetic waves. Therefore, it has become a research hotspot for many scientific researchers. Chinese patent CN201811100210.2 uses graphene oxide aqueous dispersion as a template and ethylenediamine as a nitrogen doping agent and reducing agent to prepare a nitrogen-doped reduced graphene oxide aerogel absorbing material by hydrothermal method. The minimum reflection loss can reach -67.3dB, and the effective absorption bandwidth is 3.2GHz. Chinese patent CN202210581723.X discloses a ceramic / graphene aerogel absorbing material prepared by hydrothermal reaction method, with a minimum reflection loss of -45.96dB and an effective absorption bandwidth of about 4.0GHz. However, the graphene aerogel absorbing material reported in the above patent has poor mechanical properties and is prone to structural collapse or irreversible deformation under the action of external forces, resulting in poor environmental adaptability of the material. On the other hand, the absorption band of the prepared graphene aerogel absorbing material is narrow and can only cover a specific frequency band. Summary of the invention
[0004] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a graphene aerogel absorbing material with a wide absorption band and its preparation and application, so as to overcome the problems of the existing graphene aerogel absorbing material with a narrow absorption band and poor mechanical compression performance.
[0005] The invention provides a graphene aerogel, which comprises graphene and poly(propionic anhydride); wherein the poly(propionic anhydride) connects adjacent graphene nanosheets in a bridging manner and is adsorbed on the surface of the graphene nanosheets through physical interaction forces.
[0006] The aerogel consists of graphene and poly(propionic anhydride), wherein the graphene is used as a skeleton material and the poly(propionic anhydride) is a cross-linking agent, and is prepared by thermal cross-linking of polyacrylic acid (PAA).
[0007] The poly(propionic anhydride) structural formula:
[0008] Where n=1694-4236, m=1694-4236.
[0009] The present invention provides a method for preparing a graphene aerogel, comprising:
[0010] (1) mixing graphene oxide, water and polyacrylic acid to obtain a mixed solution, and performing directional freeze drying to obtain graphene oxide aerogel;
[0011] (2) The graphene oxide aerogel is steam-reduced in a reducing agent and then heat-treated to obtain a graphite aerogel.
[0012] The preparation of graphene oxide in step (1) comprises: after graphite powder and a mixed acid of concentrated sulfuric acid / phosphoric acid are fully mixed, potassium permanganate is added in small amounts and multiple times, the temperature is raised to carry out an oxidation reaction, and after the reaction is completed, hydrogen peroxide is added, and the graphene oxide is obtained by centrifugation, washing and freeze-drying.
[0013] The preparation of graphene oxide, wherein the mesh number of the graphite powder is ≥325 mesh; the mass fraction of concentrated sulfuric acid is 95-98%, the mass fraction of phosphoric acid is ≥85%, and the volume ratio of concentrated sulfuric acid to phosphoric acid is 8:1-10:1; the mass ratio of potassium permanganate to graphite powder is 5:1-7:1; the temperature of the oxidation reaction is 35-65°C, and the reaction time is 9-13h; the mass fraction of hydrogen peroxide is ≥30%, and hydrogen peroxide is added until the solution turns golden yellow.
[0014] Preferably, in step (1), the mass ratio of graphene oxide to polyacrylic acid is 4:1 to 4:3; and the weight average molecular weight of the polyacrylic acid is 100,000-250,000.
[0015] In the step (1), graphene oxide is uniformly dispersed in deionized water, a polyacrylic acid solution is added, and the mixture is stirred to obtain a mixed solution.
[0016] Furthermore, in step (1), graphene oxide, water and polyacrylic acid are mixed: freeze-dried graphene oxide is added to water and mixed, ultrasonically dispersed in an ice water bath for 0.5-1h to obtain a graphene oxide solution, and then the polyacrylic acid solution is added and stirred for 0.5-1h to obtain a mixed solution; wherein the concentration of the graphene oxide solution is 4-6 mg / mL; and the mass percentage concentration of the polyacrylic acid solution is 25-35%.
[0017] Preferably, the directional freeze-drying in step (1) is directional freezing of the mixed solution from bottom to top.
[0018] Preferably, the directional freeze-drying: the mixed solution is frozen from bottom to top in liquid nitrogen and then freeze-dried.
[0019] For example, a glass container containing a graphene oxide / polyacrylic acid mixed solution is placed on a copper plate, and then the copper plate is immersed in liquid nitrogen (note: the copper plate must not be completely immersed in liquid nitrogen). After the sample is completely frozen, it is placed in a freeze dryer for freeze drying.
[0020] Preferably, the reducing agent in step (2) is hydrazine hydrate or hydroiodic acid.
[0021] Preferably, in step (2), the steam reduction temperature is 95-120° C. and the time is 18-24 h; and the heat treatment is vacuum heat treatment at a temperature of 160-200° C. and a time of 12-24 h.
[0022] Preferably, the mass fraction of the hydrazine hydrate is 85-98%, and the mass fraction of the hydroiodic acid is ≥45%; and the steam reduction is carried out under closed conditions.
[0023] Steam reduction: After pouring the reducing agent into a sealed glass container, put the graphene oxide aerogel in and heat it in an oven for steam reduction.
[0024] Vacuum heat treatment: For example, the aerogel after reduction by reducing agent vapor is placed in a vacuum oven, evacuated, and then heated for heat treatment.
[0025] The present invention provides an application of the graphene aerogel in the field of electromagnetic wave absorption.
[0026] Beneficial Effects
[0027] (1) The raw materials of the graphene aerogel absorbing material in the present invention are easily available, the preparation process is simple, the cost is low and the toxicity is low.
[0028] (2) The present invention adopts steam reduction and physical cross-linking methods to prepare graphene aerogel absorbing materials, avoiding the problem of poor mechanical properties caused by the traditional hydrothermal reaction method.
[0029] (3) The graphene aerogel absorbing material prepared by the present invention can achieve multi-band absorption of electromagnetic waves through mechanical compression / release, solving the problem of single absorption band of most existing graphene aerogel absorbing materials.
[0030] (4) Graphene aerogel absorbing materials have wide-band electromagnetic wave absorption behavior and have good application prospects in the field of electromagnetic wave absorption. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of the preparation of the graphene aerogel absorbing material of the present invention;
[0032] Figure 2 The Raman spectra of graphene oxide, graphene oxide aerogel and graphene aerogel in Example 1;
[0033] Figure 3 The XPS spectra of graphene oxide, graphene oxide aerogel and graphene aerogel in Example 1;
[0034] Figure 4 The high-resolution C1s spectra of graphene oxide, graphene oxide aerogel and graphene aerogel in Example 1;
[0035] Figure 5 The SEM images of the graphene aerogels in Examples 1-3 in the orthogonal directions, wherein (ac) are the SEM images of GA-1, GA-2 and GA-3 in the axial direction, and (df) are the SEM images of GA-1, GA-2 and GA-3 in the radial direction;
[0036] Figure 6 (a-c) are the relative complex dielectric constants (ε′ and ε″) and dielectric losses (tan δ ε ) curve graph;
[0037] Figure 7 (a-c) are reflection loss (RL) curves of the graphene aerogels in Examples 1-3;
[0038] Figure 8 The continuous compressive stress-strain curve and the typical cyclic compressive stress-strain curve of the graphene aerogel in the orthogonal direction in Example 1, wherein (a) and (c) are typical cyclic stress-strain curves of GA-1 in the axial direction and radial direction, respectively, and (b) and (d) are continuous compressive stress-strain curves of GA-1 in the axial direction and radial direction, respectively;
[0039] Fig. 9 (a-d) are SEM images of the graphene aerogel in Example 1 in the radial direction at different compression ratios;
[0040] Fig.10 (a-c) are the relative complex dielectric constants (ε′ and ε″) and dielectric losses (tan δ ε ) curve graph;
[0041] Fig.11 (a-d) are reflection loss (RL) curves of the graphene aerogel in Example 1 at different compression ratios;
[0042] Fig.12 This is a reflection loss (RL) curve of the graphene aerogel in Example 1 within a compression ratio range of 0-75%. DETAILED DESCRIPTION
[0043] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0044] Reagents: Graphite powder was purchased from Aladdin; hydrogen peroxide (H2O2), concentrated sulfuric acid (H2SO4), phosphoric acid (H3PO4), polyacrylic acid (PAA) solution and hydrazine hydrate (N2H4·H2O) were purchased from Sinopharm; potassium permanganate (KMnO4) was purchased from Shanghai Lingfeng Chemical Reagent Co., Ltd.
[0045] In the present invention, the instrument used to test the electromagnetic parameters of graphene aerogel is Agilent N5244A vector network analyzer. Sample preparation method: melt paraffin at 80°C, put in graphene aerogel, and then vacuum impregnate for 12 hours. After the paraffin is cooled to room temperature and solidified, the graphene aerogel impregnated with paraffin is cut into sample rings with an inner diameter of 3.04 mm, an outer diameter of 7 mm, and a thickness of 2 mm; for the test of the electromagnetic parameters of graphene aerogel under different compression ratios, the prepared graphene oxide aerogel is first compressed according to a certain ratio, and then the compressed graphene oxide aerogel is subjected to hydrazine hydrate vapor reduction and vacuum heat treatment, and finally the prepared graphene aerogel is vacuum impregnated in molten paraffin for 12 hours. After the paraffin is cooled to room temperature and solidified, the graphene aerogel impregnated with paraffin is cut into sample rings with an inner diameter of 3.04 mm, an outer diameter of 7 mm, and a thickness of 2 mm.
[0046] The absorbing performance of graphene aerogel absorbing materials is judged by reflection loss (RL) and effective absorption bandwidth (EAB), where reflection loss (RL) can be expressed as:
[0047]
[0048] In the formula, Z in and Z0 represent the impedance of the material and free space respectively, Z in It can be expressed as:
[0049]
[0050] In the formula, ε r and μ rRepresent the relative complex permittivity and relative complex permeability of the material, f is the frequency of the electromagnetic wave, d is the thickness of the material, c is the speed of the electromagnetic wave propagating in free space, ε r and μ r Can be expressed as:
[0051] ε r =ε′jε″
[0052] μ r =μ′-jμ″
[0053] Wherein, ε′ and ε″ represent the real and imaginary parts of the relative complex permittivity, and μ′ and μ″ represent the real and imaginary parts of the relative complex permeability, respectively.
[0054] The effective absorption bandwidth (EAB) refers to the frequency range where the reflection loss (RL) value is ≤-10dB.
[0055] Example 1
[0056] (1) Weigh 3 g of graphite powder in a 1000 mL three-necked flask, slowly pour a mixed acid of 360 mL of concentrated sulfuric acid and 40 mL of phosphoric acid into the flask, and pre-oxidize at 0° C. for 30 min; then weigh 18 g of potassium permanganate and add it to the mixed system in small amounts and multiple times; heat to 50° C. and react for 10 h; after the reaction is completed, slowly pour the mixture into 400 mL of deionized water, and add 30% hydrogen peroxide drop by drop until the solution turns golden yellow; finally, wash repeatedly with deionized water until the pH value of the supernatant is close to 7, and freeze-dry to obtain graphene oxide;
[0057] (2) 50 mg of graphene oxide was added to 10 mL of deionized water, and ultrasonically dispersed in an ice-water bath for 1 h. Then, a polyacrylic acid solution with a weight average molecular weight of 240,000 was added in a ratio of 4:1 between graphene oxide and polyacrylic acid, and magnetic stirring was performed for 1 h. Finally, the fully mixed graphene oxide / polyacrylic acid solution was directionally frozen in liquid nitrogen (the specific operation is as follows: the mixed solution was poured into a mold and placed on a copper plate, and then the copper plate was immersed in liquid nitrogen (note: the copper plate should not be completely immersed in liquid nitrogen), and slowly directionally frozen from bottom to top), and placed in a freeze dryer for freeze drying to obtain graphene oxide aerogel;
[0058] (3) 15 mL of 85% hydrazine hydrate was added to a 2000 mL sealed glass container, and graphene oxide aerogel was placed in the container. The temperature was raised to 95°C in an oven, and the aerogel was steam-reduced for 24 hours. Then, the aerogel reduced by hydrazine hydrate steam was thermally cross-linked in a vacuum oven at 160°C for 24 hours to obtain graphene aerogel (GA-1).
[0059] Example 2
[0060] (1) Weigh 3 g of graphite powder in a 1000 mL three-necked flask, slowly pour a mixed acid of 360 mL of concentrated sulfuric acid and 40 mL of phosphoric acid into the flask, and pre-oxidize at 0° C. for 30 min; then weigh 18 g of potassium permanganate and add it to the mixed system in small amounts and multiple times; heat to 50° C. and react for 10 h; after the reaction is completed, slowly pour the mixture into 400 mL of deionized water, and add 30% hydrogen peroxide drop by drop until the solution turns golden yellow; finally, wash repeatedly with deionized water until the pH value of the supernatant is close to 7, and freeze-dry to obtain graphene oxide;
[0061] (2) 50 mg of graphene oxide was added to 10 mL of deionized water, and ultrasonically dispersed in an ice-water bath for 1 h. Then, a polyacrylic acid solution with a weight average molecular weight of 240,000 was added in a ratio of 2:1 between graphene oxide and polyacrylic acid, and magnetic stirring was performed for 1 h. Finally, the fully mixed graphene oxide / polyacrylic acid solution was directionally frozen in liquid nitrogen (the specific operation is as follows: the mixed solution was poured into a mold and placed on a copper plate, and then the copper plate was immersed in liquid nitrogen (note: the copper plate should not be completely immersed in liquid nitrogen), and slowly directionally frozen from bottom to top), and then placed in a freeze dryer for freeze drying to obtain graphene oxide aerogel;
[0062] (3) 15 mL of 85% hydrazine hydrate was added to a 2000 mL sealed glass container, and graphene oxide aerogel was placed in the container. The temperature was raised to 95°C in an oven, and the aerogel was steam-reduced for 24 hours. Then, the aerogel reduced by hydrazine hydrate steam was thermally cross-linked in a vacuum oven at 160°C for 24 hours to obtain graphene aerogel (GA-2).
[0063] Example 3
[0064] (1) Weigh 3 g of graphite powder in a 1000 mL three-necked flask, slowly pour a mixed acid of 360 mL of concentrated sulfuric acid and 40 mL of phosphoric acid into the flask, and pre-oxidize at 0° C. for 30 min; then weigh 18 g of potassium permanganate and add it to the mixed system in small amounts and multiple times; heat to 50° C. and react for 10 h; after the reaction is completed, slowly pour the mixture into 400 mL of deionized water, and add 30% hydrogen peroxide drop by drop until the solution turns golden yellow; finally, wash repeatedly with deionized water until the pH value of the supernatant is close to 7, and freeze-dry to obtain graphene oxide;
[0065] (2) 50 mg of graphene oxide was added to 10 mL of deionized water, and ultrasonically dispersed in an ice-water bath for 1 h. Then, a polyacrylic acid solution with a weight average molecular weight of 240,000 was added in a mass ratio of 4:3 between graphene oxide and polyacrylic acid, and magnetic stirring was performed for 1 h. Finally, the fully mixed graphene oxide / polyacrylic acid solution was directionally frozen in liquid nitrogen (the specific operation is as follows: the mixed solution was poured into a mold and placed on a copper plate, and then the copper plate was immersed in liquid nitrogen (note: the copper plate should not be completely immersed in liquid nitrogen), and slowly directionally frozen from bottom to top), and placed in a freeze dryer for freeze drying to obtain graphene oxide aerogel;
[0066] (3) 15 mL of 85% hydrazine hydrate was added to a 2000 mL sealed glass container, and graphene oxide aerogel was placed in the container. The temperature was raised to 95°C in an oven, and the aerogel was steam-reduced for 24 hours. Then, the aerogel reduced by hydrazine hydrate steam was thermally cross-linked in a vacuum oven at 160°C for 24 hours to obtain graphene aerogel (GA-3).
[0067] The preparation process of graphene aerogel absorbing materials is as follows: Figure 1 As shown. First, the graphene oxide prepared by the Hummers method and the polyacrylic acid solution are fully mixed to allow the polyacrylic acid molecules to adsorb on the surface of the graphene oxide nanosheets; then, the uniformly mixed graphene oxide / polyacrylic acid mixed solution is directionally frozen in liquid nitrogen and then placed in a freeze dryer for freeze drying; finally, the freeze-dried graphene oxide aerogel is reduced in hydrazine hydrate vapor and then heat treated in a vacuum environment to obtain graphene aerogel.
[0068] like Figure 2 The Raman spectra of graphene oxide, graphene oxide aerogel and graphene aerogel in Example 1 are shown. All materials have two significant characteristic peaks, namely the D band and the G band. The intensity ratio of the D band to the G band (I D / I G ) is used to indicate the degree of graphitization and defects of the material. D / I G The values are similar, indicating that the degree of defects of the two are almost the same. After hydrazine hydrate vapor reduction and vacuum heat treatment, I D / I G The value increases to 1.03, indicating that more defects are introduced into the material. The increase in defects will lead to an increase in the number of dipoles. Under the action of electromagnetic waves, the dipole polarization will be enhanced, thereby promoting the attenuation of electromagnetic waves.
[0069] like Figure 3Shown are XPS spectra of graphene oxide, graphene oxide aerogel and graphene aerogel in Example 1. All materials show significant C1s and O1s characteristic peaks. Compared with graphene oxide, the addition of polyacrylic acid slightly increases the intensity ratio of C1s and O1s peaks. After hydrazine hydrate vapor reduction and vacuum heat treatment, the intensity ratio of C1s and O1s peaks increases to 5.41, indicating that a large amount of O element is removed.
[0070] like Figure 4 Shown are high-resolution C1s spectra of graphene oxide, graphene oxide aerogel and graphene aerogel in Example 1. After hydrazine hydrate vapor reduction and vacuum heat treatment, the intensity ratio of the C=C / CC bond and the characteristic peak containing O bonds increases, indicating that the graphene oxide is effectively reduced.
[0071] like Figure 5 The graphene aerogels in the orthogonal directions are shown in Figure 1-3. The graphene aerogels have an anisotropic microstructure, showing a wavy hierarchical structure, and the layers are connected by "bridges".
[0072] like Figure 6 The relative complex dielectric constants (ε′ and ε″) and dielectric losses (tan δ ε ) curve. The relative dielectric constant and dielectric loss of graphene aerogel show a downward trend in the entire frequency range, and with the increase of polyacrylic acid content, the relative complex dielectric constant and dielectric loss gradually decrease. When the mass ratio of graphene oxide to polyacrylic acid is 4:1, ε′ and ε″ decrease from 4.57 and 2.04 to 3.37 and 0.89 respectively in the entire frequency range, and tanδ ε When the mass ratio of graphene oxide to polyacrylic acid increases to 4:3, ε′ and ε″ decrease from 3.64 and 1.54 to 2.79 and 0.26, respectively, over the entire frequency range, and tanδ ε It also decreased from 0.42 to 0.09.
[0073] like Figure 7 The graphene aerogel reflection loss (RL) curves of Examples 1-3 are shown. When the mass ratio of graphene oxide to polyacrylic acid is 4:1, the minimum reflection loss of the graphene aerogel is -13.7 dB, and the effective absorption bandwidth is 2.7 GHz. As the content of polyacrylic acid increases, the wave absorption performance of the graphene aerogel gradually decreases. When the mass ratio of graphene oxide to polyacrylic acid is 4:3, the minimum reflection loss is only -5.6 dB.
[0074] like Figure 8The graphs show typical cyclic compression stress-strain curves and continuous compression stress-strain curves of the graphene aerogel in the orthogonal directions in Example 1. When the compression ratio is 50%, the maximum compression strengths of the graphene aerogel in the axial direction and radial direction are 7.8 KPa and 3.2 KPa, respectively. Even after 20 compression cycles, the compression strengths can still be maintained at 69.2% and 75.0%, respectively. As the compression ratio increases, the maximum compression strengths of the graphene aerogel in the axial direction and radial direction both show an increasing trend, and can withstand a compression ratio of 80%.
[0075] like Fig. 9 The graphene aerogel in the radial direction at different compression ratios is shown in Figure 1. As the compression ratio increases, the structure of the graphene aerogel becomes denser, which is beneficial to the transition of electrons and the scattering of electromagnetic waves, and enhances the attenuation of electromagnetic waves.
[0076] like Fig.10 The relative complex dielectric constant (ε′ and ε″) and dielectric loss (tan δ ε ) curve. When the graphene aerogel is not compressed, ε′ and ε″ decrease from 4.57 and 2.04 to 3.37 and 0.89 respectively in the entire frequency range, and tanδ ε It also decreased from 0.45 to 0.26. With the increase of compression ratio, the relative complex dielectric constant and dielectric loss of graphene aerogel both showed an increasing trend. When the compression ratio increased to 75%, ε′ and ε" decreased from 7.45 and 3.53 to 5.2 and 2.82 respectively in the entire frequency range, and tanδ ε It fluctuates between 0.47 and 0.57.
[0077] like Fig.11 The graph shows the reflection loss (RL) curve of the graphene aerogel at different compression ratios in Example 1. When the graphene aerogel is not compressed, the minimum reflection loss is -13.7dB and the effective absorption bandwidth is 2.7GHz. As the compression ratio increases, the absorption efficiency gradually increases. When the compression ratio increases to 75%, the minimum reflection loss can reach -42.8dB and the effective absorption bandwidth is 5.7GHz.
[0078] like Fig.12 The graph shows the reflection loss (RL) curve of the graphene aerogel in the compression ratio range of 0-75% in Example 1. The minimum reflection loss and effective absorption bandwidth of the graphene aerogel can be adjusted by adjusting the compression ratio. In the compression ratio range of 0-75%, the effective absorption bandwidth of the graphene aerogel can cover 12.0 GHz, proving that adjusting the compression strain can adjust the absorption intensity and effective absorption bandwidth, and can achieve multi-band absorption of electromagnetic waves.
Claims
1. A graphene aerogel, characterized in that: The graphene aerogel comprises graphene and poly(propionic anhydride); wherein the poly(propionic anhydride) connects adjacent graphene nanosheets in a bridging manner and is adsorbed on the surface of the graphene nanosheets.
2. The graphene aerogel material according to claim 1, characterized in that: The poly(propionic anhydride) structural formula: Where n=1694-4236, m=1694-4236.
3. A method for preparing graphene aerogel, comprising: (1) mixing graphene oxide, water and polyacrylic acid to obtain a mixed solution, and performing directional freeze drying to obtain graphene oxide aerogel; (2) The graphene oxide aerogel is steam-reduced in a reducing agent and then heat-treated to obtain a graphite aerogel.
4. The preparation method according to claim 3, characterized in that: In the step (1), the mass ratio of graphene oxide to polyacrylic acid is 4:1 to 4:3; and the weight average molecular weight of the polyacrylic acid is 100,000-250,000.
5. The preparation method according to claim 3, characterized in that: In the step (1), graphene oxide, water and polyacrylic acid are mixed: graphene oxide and water are mixed, ultrasonically dispersed in an ice water bath to obtain a graphene oxide solution, and then the polyacrylic acid solution is added and stirred to obtain a mixed solution; wherein the concentration of the graphene oxide solution is 4-6 mg / mL; and the mass percentage concentration of the polyacrylic acid solution is 25-35%.
6. The preparation method according to claim 3, characterized in that: The directional freeze-drying in step (1) is the directional freezing of the mixed solution from bottom to top.
7. The preparation method according to claim 6, characterized in that: The directional freeze drying: the mixed solution is frozen from bottom to top in liquid nitrogen and then freeze-dried.
8. The preparation method according to claim 3, characterized in that: The reducing agent in step (2) is hydrazine hydrate or hydroiodic acid; the steam reduction temperature in step (2) is 95-120° C. and the time is 18-24 hours; the heat treatment is vacuum heat treatment at a temperature of 160-200° C. and a time of 12-24 hours.
9. The preparation method according to claim 8, characterized in that: The concentration of the hydrazine hydrate is 85-98%, and the concentration of the hydroiodic acid is ≥45%; and the steam reduction is carried out under closed conditions.
10. Use of the graphene aerogel according to claim 1 in the field of electromagnetic wave absorption.
Citation Information
Patent Citations
Method for preparing nitrogen doped reduced graphene oxide aerogel wave-absorbing material
CN108946711A
Ceramic / graphene aerogel wave-absorbing material as well as preparation method and application thereof
CN114853502A
Graphene aerogel microspheres and preparation method thereof
CN106185908A
Preparation method of graphene composite aerogel absorbing material and application thereof
CN107399735A
High polymer composite graphene aerogel and composite phase change material prepared from high polymer composite graphene aerogel
CN116004188A
Cited By
Preparation method and application of adjustable reduced graphene oxide broadband wave-absorbing material