Coal tar-based oxygen-enriched porous capacitor carbon as well as preparation method and application thereof

By pre-oxidizing and high-temperature carbonizing coal tar and alkaline earth metal or alkali metal hydroxide as activators, oxygen-rich porous capacitive carbon is prepared, which solves the problems of high energy consumption and environmental pollution in the preparation of coal tar porous carbon in the existing technology. , achieving high specific surface area and excellent energy storage performance, supporting large-scale industrial production.

CN118754122APending Publication Date: 2024-10-11XINJIANG UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410932768.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing method of preparing porous carbon using coal tar as raw material has the problems of high energy consumption, complex process, low output and environmental pollution, and it is difficult to achieve large-scale industrial production.

Method used

By mixing coal tar with alkaline earth metal or alkali metal hydroxide as an activator, pre-oxidation and high-temperature carbonization are performed to prepare oxygen-rich porous capacitive carbon, which avoids the secondary treatment of coal tar, simplifies the process flow, and reduces the cost. costs and improve productivity.

Benefits of technology

The high specific surface area and excellent energy storage performance of coal tar-based oxygen-rich porous capacitive carbon are achieved, supporting the provision of high specific capacitance of more than 400F/g and good cycle stability under high load, and has the potential for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754122A_ABST
    Figure CN118754122A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of advanced functional materials, and particularly relates to coal tar-based oxygen-enriched porous capacitor carbon as well as a preparation method and application thereof. The coal tar-based oxygen-enriched porous carbon with high specific surface area and rich micropores and mesopores is prepared by adopting a pre-oxidation-carbonization method, taking coal tar as a carbon source, taking alkaline earth metal or hydroxide or carbonate of alkali metal as an activating agent, pre-oxidizing the coal tar and then carbonizing the coal tar at high temperature. The oxygen-enriched porous carbon has rich oxygen-containing functional groups, ultrahigh specific surface area and proper pore size distribution, and when the oxygen-enriched porous carbon is applied to a supercapacitor, the high specific capacitance of 400F / g or above and good cycling stability are still achieved under the ultrahigh loading capacity 2.5 times higher than commercial loading capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of advanced functional materials, and in particular relates to a coal tar-based oxygen-enriched porous capacitor carbon and a preparation method and application thereof. Background Art

[0002] Porous carbon is a carbon material with a rich pore structure, usually including micropores (<2nm), mesopores (2nm~50nm) and macropores (>50nm). It has the advantages of high specific surface area, good conductivity, chemical stability and high mechanical strength. These properties make it have broad application prospects in energy storage, separation, catalysis, medical treatment and other aspects. There are many methods for preparing porous carbon, the common ones include hard template method, soft template method and self-assembly method. The hard template method is a commonly used method for preparing porous carbon. Its basic principle is to use the pore structure of the hard template as a template to form a porous carbon structure after pyrolysis of the carbon precursor. The hard template usually selects potassium hydroxide, silica, aluminum oxide and other materials. By washing, pyrolysis and other steps to remove the hard template, a porous carbon material with a rich pore structure can be obtained. The soft template method is another common method for preparing porous carbon, which is characterized by using the pore structure of the soft template to prepare porous carbon materials. The soft template can be polystyrene microspheres, polymer colloids and other materials. Through the process of dispersion, pyrolysis and removal of the soft template, a porous carbon material with a specific pore structure can be obtained. The self-assembly method uses the characteristics of molecular self-assembly to form an ordered structure in the solution, and then forms a porous carbon structure after pyrolysis. Among them, the hard template method is widely used because of its simple operation, cheap and easy-to-obtain raw materials, and the ability to direct the synthesis of carbon materials with various morphologies and structures.

[0003] The carbon sources for preparing porous carbon mainly include natural organic matter such as lignin, cotton stalks, corn stalks, houttuynia cordata, polystyrene, polyacrylates and synthetic polymers. Although this type of natural organic matter is easy to obtain, it cannot be used as a raw material for large-scale production of porous carbon due to the limitations of origin and output. Synthetic polymers are not restricted by origin and can be produced on a large scale, but their high energy consumption and high production costs limit their application. Coal tar is a primary product produced by the pyrolysis process of coal in the coal chemical process. It is rich in a large number of polycyclic aromatic hydrocarbons, has a high carbon content, low ash content, high output, and is cheap and easy to obtain. It is an ideal raw material for preparing porous carbon. However, the traditional coal tar deep processing industry has high energy consumption, complex processes, low output, and serious environmental pollution. Therefore, how to achieve high value-added utilization of coal tar is a major issue that needs to be solved, among which converting coal tar into high-performance carbon materials is an important direction for its high value-added green utilization.

[0004] At present, in the method of preparing porous carbon from coal tar, researchers have used zinc acetate (Chen Zhang, Weihao Zhang, Moxin Yu*, Kemeng Ning, Li Zhang, Xiaoting Wang, Xiaojun He*, Synthesis of hollow porous carbon nanospheres from coal tar for adsorption of Direct Black 38dye, J. Porous Mater, 2017, 24, 1289-1293), ionic liquid (Xiaoyu Xie, Xiaojun He*, Hanfang Zhang, Feng Wei, Nan Xiao, Jieshan Qiu, Interconnected sheet-like porous carbons from coal tar by a confined soft-template strategy for supercapacitors, Chem. Eng. J. 2018, 350, 49-56), molten salt (Huichao Liu, Hua Song, Wenjing Hou, Yunzhen Chang, Ying Zhang, Yanping Li, Yun Zhao, Gaoyi Han*, Coal tarpitch-based Hierarchical porous carbons prepared in molten salt for supercapacitors, Mater. Chem. Phys, 2021, 265, 124491.) was used as a template to prepare a series of porous carbons using the high carbon content and strong plasticity of coal tar, and applied them to energy storage. In these methods, coal tar needs to be pre-treated, and the template dosage used is large, the raw materials are expensive, and the reaction conditions are harsh, making it difficult to mass-produce industrial products. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a coal tar-based oxygen-enriched porous capacitor carbon and a preparation method and application thereof. In the method, the coal tar does not require secondary treatment, the method is simple, the cost is low, and the yield is high. The prepared coal tar-based oxygen-enriched porous capacitor carbon is oxygen-enriched and porous, has a high specific surface area, and has excellent energy storage performance.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing coal tar-based oxygen-enriched porous capacitor carbon, comprising the following steps:

[0008] The coal tar and the activator are mixed and pre-oxidized to obtain a pre-oxidized material;

[0009] Carbonizing the pre-oxidized material at high temperature in a protective atmosphere to obtain coal tar-based oxygen-rich porous capacitor carbon;

[0010] The activator includes one or more of alkaline earth metal hydroxides, alkaline earth metal carbonates, alkali metal hydroxides, alkali metal carbonates and alkali metal bicarbonates;

[0011] The pre-oxidation is carried out in an atmosphere with an oxygen volume content of 5 to 20%;

[0012] The temperature of the high temperature carbonization is 500-900°C.

[0013] Preferably, the alkaline earth metal includes calcium and / or magnesium; and the alkali metal includes potassium and / or sodium.

[0014] Preferably, the mass ratio of the coal tar to the activator is 1:0.5-4.

[0015] Preferably, the pre-oxidation temperature is 150-450° C., and the holding time is 0.5-3.5 h.

[0016] Preferably, the high temperature carbonization holding time is 1 to 5 hours.

[0017] Preferably, the protective atmosphere includes nitrogen, argon or helium; the flow rate of the protective atmosphere is 10 to 200 mL / min.

[0018] Preferably, the heating rate to the high-temperature carbonization temperature is 1 to 10° C. / min.

[0019] Preferably, after the high-temperature carbonization, the process further comprises: washing and drying the product of the high-temperature carbonization in sequence; the washing comprises washing with water until neutral after acid leaching, or directly washing with water.

[0020] The present invention also provides a coal tar-based oxygen-enriched porous capacitor carbon prepared by the preparation method described in the above technical scheme, wherein the oxygen mass percentage of the coal tar-based oxygen-enriched porous capacitor carbon is 5-25%, the pore diameter is 0.5-20nm, and the porosity is 0.5-2cm 3 / g, specific surface area ≥2000m 2 / g.

[0021] The present invention also provides the use of the coal tar-based oxygen-rich porous capacitor carbon described in the above technical solution in a supercapacitor.

[0022] The invention provides a method for preparing coal tar-based oxygen-enriched porous capacitor carbon, comprising the following steps: coal tar and an activator are mixed and pre-oxidized to obtain a pre-oxidized material; the pre-oxidized material is carbonized at high temperature in a protective atmosphere to obtain the coal tar-based oxygen-enriched porous capacitor carbon; the activator comprises one or more of alkaline earth metal hydroxides, alkaline earth metal carbonates, alkali metal hydroxides, alkali metal carbonates and alkali metal bicarbonates; the pre-oxidation is carried out in an atmosphere with an oxygen volume content of 5 to 20%; and the temperature of the high-temperature carbonization is 500 to 900°C.

[0023] The present invention mixes cheap coal tar without any treatment with an activator, and prepares a coal tar-based oxygen-enriched porous capacitor carbon with rich oxygen-containing functional groups, high specific surface area, rich micropores and mesopores by controlling the oxygen content in the atmosphere during the pre-oxidation process and the high-temperature carbonization temperature. The coal tar is applied to supercapacitors, and still has a high specific capacitance of more than 400F / g and good cycle stability at an ultra-high load of 2.5 times higher than the commercial load. In the method, coal tar does not need secondary treatment, the method is simple and easy to carry out mass production, the raw material source is wide, the price is low, the cost is low, and the yield is high. The prepared coal tar-based oxygen-enriched porous capacitor carbon is oxygen-enriched and porous, has a high specific surface area, and has excellent energy storage performance, and is easy to realize industrial production. At the same time, it provides new ideas and new ways for the high value-added utilization of coal tar. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a physical picture of the coal tar-based oxygen-enriched porous capacitor carbon prepared in Example 1;

[0025] Figure 2 This is a SEM image of the coal tar-based oxygen-enriched porous capacitor carbon prepared in Example 1;

[0026] Figure 3 The coal tar-based oxygen-rich porous capacitor carbon (Y x CK) and the cyclic voltammetry (CV) diagram of the commercial activated carbon (YP-50F) of Comparative Example 1;

[0027] Figure 4 The coal tar-based oxygen-rich porous capacitor carbon (Y x CK) and constant current charge and discharge (GCD) diagram of commercial activated carbon (YP-50F) of comparative example 1. DETAILED DESCRIPTION

[0028] The present invention provides a method for preparing coal tar-based oxygen-enriched porous capacitor carbon, comprising the following steps:

[0029] The coal tar and the activator are mixed and pre-oxidized to obtain a pre-oxidized material;

[0030] Carbonizing the pre-oxidized material at high temperature in a protective atmosphere to obtain coal tar-based oxygen-rich porous capacitor carbon;

[0031] The activator includes one or more of alkaline earth metal hydroxides, alkaline earth metal carbonates, alkali metal hydroxides, alkali metal carbonates and alkali metal bicarbonates;

[0032] The pre-oxidation is carried out in an atmosphere with an oxygen volume content of 5 to 20%;

[0033] The temperature of the high temperature carbonization is 500-900°C.

[0034] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used in the preparation, and commercially available products known to those skilled in the art can be used.

[0035] The invention mixes coal tar and an activator, performs pre-oxidation, and obtains a pre-oxidation material.

[0036] In the present invention, the activator includes one or more of alkaline earth metal hydroxides, alkaline earth metal carbonates, alkali metal hydroxides, alkali metal carbonates and alkali metal bicarbonates, preferably alkaline earth metal hydroxides or alkali metal hydroxides; the alkaline earth metal preferably includes calcium and / or magnesium, more preferably calcium; the alkali metal preferably includes potassium and / or sodium, more preferably potassium; the activator is most preferably potassium hydroxide, sodium hydroxide, calcium hydroxide, magnesium hydroxide, potassium carbonate or potassium bicarbonate.

[0037] The activator in the present invention plays a role in removing amorphous carbon and surface functional groups during the preparation of the carbon material, thereby increasing the porosity and specific surface area of ​​the carbon material. Compared with other activators, the metal ions in the hydroxide of the alkali metal can react with the functional groups on the surface of the carbon material to generate water-soluble metal salts, thereby increasing the surface activity of the carbon material.

[0038] In the present invention, the mass ratio of the coal tar to the activator is preferably 1:0.5-4, more preferably 1:0.5-2.

[0039] In the present invention, the coal tar and the activator are preferably mixed under stirring conditions at room temperature; the stirring rate is preferably 200 to 800 rpm, more preferably 200 to 400 rpm; the stirring time is preferably 10 to 60 minutes, more preferably 30 to 50 minutes. The present invention allows the coal tar to be uniformly coated with the activator by stirring.

[0040] In the present invention, the pre-oxidation temperature is preferably 150-450°C, more preferably 200-400°C, and the holding time is preferably 0.5-3.5h, more preferably 1-2h; the pre-oxidation is carried out in an atmosphere with an oxygen volume content of 5-20%, preferably air, or a mixed atmosphere of oxygen and nitrogen with an oxygen volume percentage of 5-10%.

[0041] During the pre-oxidation process, coal tar is cross-linked and the side chain groups are oxidized to generate oxygen-containing functional groups.

[0042] After obtaining the pre-oxidation material, the present invention performs high-temperature carbonization on the pre-oxidation material in a protective atmosphere to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0043] In the present invention, the temperature of the high-temperature carbonization is 500-900°C, preferably 700-800°C; the holding time of the high-temperature carbonization is preferably 1-5h, more preferably 2-4h; the heating rate to the high-temperature carbonization temperature is preferably 1-10°C / min, more preferably 2-5°C / min; the protective atmosphere preferably includes nitrogen, argon or helium, more preferably nitrogen; the flow rate of the protective atmosphere is preferably 10-200mL / min, more preferably 30-80mL / min.

[0044] During the high-temperature carbonization process, the small molecules in the coal tar that have not undergone cross-linking absorb heat and volatilize, forming a large number of gas pathways. At the same time, the activator etches the carbon material, thereby forming an oxygen-rich porous capacitor carbon with a high specific surface area and suitable pore size distribution.

[0045] After the high temperature carbonization, the present invention preferably further comprises: washing and drying the product of the high temperature carbonization in sequence; the washing is preferably washing with water to neutrality after acid leaching, or directly washing with water, more preferably washing with water to neutrality after acid leaching; the acid used for the acid leaching is preferably hydrochloric acid; the concentration of the hydrochloric acid is preferably 1-3 mol / L, more preferably 1.5-2.5 mol / L; the time of the acid leaching is preferably 2-3h, more preferably 2h; the water is preferably distilled water; the drying temperature is preferably 60-80°C, more preferably 60-70°C; the drying time is preferably 3-6h, more preferably 5h. The present invention removes the residual activator by washing.

[0046] The present invention adopts a pre-oxidation-carbonization method, uses coal tar as a carbon source, and hydroxides or carbonates of alkaline earth metals or alkali metals as activators. The coal tar is first pre-oxidized and then carbonized at high temperature to prepare a coal tar-based oxygen-enriched porous carbon with a high specific surface area, abundant micropores and mesopores. The oxygen-enriched porous carbon has abundant oxygen-containing functional groups, ultra-high specific surface area and suitable pore size distribution. When applied to supercapacitors, it still has a high specific capacitance of more than 400F / g and good cycle stability at an ultra-high load that is 2.5 times higher than the commercial load.

[0047] The present invention also provides a coal tar-based oxygen-enriched porous capacitor carbon prepared by the preparation method described in the above technical scheme, wherein the oxygen mass percentage of the coal tar-based oxygen-enriched porous capacitor carbon is 5-25%, the pore diameter is 0.5-20nm, and the porosity is 0.5-2cm 3 / g, specific surface area ≥2000m 2 / g.

[0048] In the present invention, the oxygen mass percentage of the coal tar-based oxygen-enriched porous capacitor carbon is preferably 15-20%, the pore size is preferably 0.5-8 nm, and the porosity is preferably 1-1.5 cm 3 / g, and the specific surface area is preferably 2200 to 3000m 2 / g.

[0049] The present invention also provides the use of the coal tar-based oxygen-rich porous capacitor carbon described in the above technical solution in a supercapacitor.

[0050] The present invention has no special limitation on the application of the coal tar-based oxygen-rich porous capacitor carbon in supercapacitors, and any application method known in the art can be used.

[0051] In the application example of the present invention, the supercapacitor is specifically a symmetrical supercapacitor; the preparation method of the symmetrical supercapacitor is specifically as follows: the coal tar-based oxygen-rich porous capacitor carbon and acetylene black are added to a mortar containing anhydrous ethanol, and then a polytetrafluoroethylene dispersion is added for grinding, and the obtained ground mixture is adhered to a nickel mesh and dried to obtain an electrode sheet; the electrode sheet and the electrolyte are assembled to obtain a symmetrical supercapacitor; the size of the nickel mesh is 1 cm×1 cm×0.1 cm; the adhesion amount of the ground mixture on the nickel mesh is 25 mg / cm 2 ; The drying temperature is 60°C; The drying time is 12h; The drying equipment is a vacuum drying oven; The electrolyte is a KOH solution; The concentration of the KOH solution is 6mol / L.

[0052] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.

[0053] Example 1

[0054] Accurately weigh 2.0g of coal tar and 1.0g of KOH and place them in a 25mL beaker, stir at 300rpm for 30min at room temperature to mix the coal tar and KOH evenly, then transfer them to a magnetic boat (6cm×3cm×2cm), put them in a muffle furnace, and pre-oxidize them at 150°C for 1h in nitrogen with an oxygen volume content of 5%. Then transfer the pre-oxidized material to a tubular furnace and heat it to 700°C at a heating rate of 2°C / min in nitrogen (flow rate of 20mL / min) for 2h for high-temperature carbonization. After natural cooling, soak it in 1mol / L hydrochloric acid for 2h, wash it with distilled water until it is neutral, and put it in an oven to dry at 70°C for 4h to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0055] Example 2

[0056] Accurately weigh 2.0g of coal tar and 1.0g of KOH and place them in a 25mL beaker, stir at 600rpm for 30min at room temperature to mix the coal tar and KOH evenly, then transfer them to a magnetic boat (6cm×3cm×2cm), put them in a muffle furnace, and pre-oxidize them at 200℃ for 2h in nitrogen with an oxygen volume content of 10%. Then transfer the pre-oxidized material to a tubular furnace and heat it to 700℃ at a heating rate of 5℃ / min in nitrogen (flow rate of 150mL / min) for 2h for high-temperature carbonization. After natural cooling, soak it in 3mol / L hydrochloric acid for 2h, wash it with distilled water until it is neutral, and put it in an oven to dry at 60℃ for 3h to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0057] Example 3

[0058] Accurately weigh 2.0g coal tar and 1.0g KOH and place them in a 25mL beaker, stir at 800rpm for 30min at room temperature to mix the coal tar and KOH evenly, then transfer them to a magnetic boat (6cm×3cm×2cm), put them in a muffle furnace, and pre-oxidize them at 200℃ for 2h in nitrogen with an oxygen volume content of 10%. Then transfer the pre-oxidized material to a tubular furnace and heat it to 700℃ at a heating rate of 5℃ / min in nitrogen (flow rate of 200mL / min) for 2h for high-temperature carbonization. After natural cooling, soak it in 1.5mol / L hydrochloric acid for 2h, wash it with distilled water until it is neutral, put it in an oven and dry it at 70℃ for 6h to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0059] Example 4

[0060] Accurately weigh 2.0 g of coal tar and 1.0 g of KOH and place them in a 25 mL beaker. Stir at 400 rpm for 30 min at room temperature to evenly mix the coal tar and KOH. Then transfer them to a magnetic boat (6 cm × 3 cm × 2 cm) and put them in a muffle furnace. Pre-oxidize them at 400 °C in air for 2 h. Then transfer the pre-oxidized material to a tubular furnace and heat it to 700 °C at a heating rate of 5 °C / min in nitrogen (flow rate of 80 mL / min) for 2 h for high-temperature carbonization. After natural cooling, soak it in 2 mol / L hydrochloric acid for 2 h, wash it with distilled water until it is neutral, and put it in an oven to dry it at 65 °C for 5 h to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0061] Example 5

[0062] Accurately weigh 2.0 g of coal tar and 1.0 g of KOH and place them in a 25 mL beaker. Stir at 500 rpm for 30 min at room temperature to evenly mix the coal tar and KOH. Then transfer them to a magnetic boat (6 cm × 3 cm × 2 cm) and put them in a muffle furnace. Pre-oxidize them at 350 ° C in air for 2 h. Then transfer the pre-oxidized material to a tubular furnace and heat it to 800 ° C at a heating rate of 5 ° C / min in nitrogen (flow rate of 70 mL / min) for 2 h for high-temperature carbonization. After natural cooling, soak it in 2.5 mol / L hydrochloric acid for 2 h, wash it with distilled water until neutral, and put it in an oven to dry at 75 ° C for 4 h to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0063] Example 6

[0064] Accurately weigh 2.0 g of coal tar and 1.0 g of NaOH and place them in a 25 mL beaker. Stir at 600 rpm for 30 min at room temperature to evenly mix the coal tar and NaOH. Then transfer them to a magnetic boat (6 cm × 3 cm × 2 cm) and put them in a muffle furnace. Pre-oxidize them at 280 ° C in air for 2 h. Then transfer the pre-oxidized material to a tubular furnace and heat it to 800 ° C at a heating rate of 5 ° C / min in nitrogen (flow rate of 90 mL / min) for 2 h for high-temperature carbonization. After natural cooling, soak it in 3 mol / L hydrochloric acid for 2 h, wash it with distilled water until neutral, and put it in an oven to dry at 80 ° C for 4 h to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0065] Example 7

[0066] Accurately weigh 2.0g coal tar and 1.0g Na2CO3 and place them in a 25mL beaker, stir at 600rpm for 30min at room temperature to mix the coal tar and Na2CO3 evenly, then transfer them to a magnetic boat (6cm×3cm×2cm), put them in a muffle furnace, and pre-oxidize them at 420℃ in air for 2h. Then transfer the pre-oxidized material to a tubular furnace and heat it to 800℃ at a heating rate of 5℃ / min in nitrogen (flow rate of 60mL / min) for 2h for high-temperature carbonization. After natural cooling, soak it in 1.5mol / L hydrochloric acid for 2h, wash it with distilled water until it is neutral, put it in an oven and dry it at 60℃ for 5h to obtain coal tar-based oxygen-enriched porous capacitor carbon.

[0067] Comparative Example 1

[0068] Commercial activated carbon (YP-50F) was used as a comparative example.

[0069] Application Example 1

[0070] The coal tar-based oxygen-enriched porous capacitor carbon prepared in Example 1 was used for supercapacitors. The specific preparation process was as follows: the coal tar-based oxygen-enriched porous capacitor carbon, acetylene black and polytetrafluoroethylene dispersion were weighed in a mass ratio of 8:1:1, and then the active substance and acetylene black were added to a mortar filled with anhydrous ethanol, and then the polytetrafluoroethylene dispersion was added and fully ground. The ground mixture (25 mg / cm 2 , 1cm×1cm×0.1cm) was adhered to a nickel mesh and placed in a vacuum drying oven at 60°C for 12h to obtain an electrode sheet, which was assembled into a symmetrical supercapacitor with a 6mol / L KOH solution as the electrolyte.

[0071] The obtained symmetric supercapacitor was tested for its supercapacitor performance under a load condition that is 2.5 times that of the commercial load.

[0072] Application Examples 2 to 7

[0073] The difference from Application Example 1 is that the coal tar-based oxygen-enriched porous capacitor carbon prepared in Example 1 is replaced by the coal tar-based oxygen-enriched porous capacitor carbon prepared in Examples 2 to 7 respectively.

[0074] Comparative application example 1

[0075] The difference from Application Example 1 is that the coal tar-based oxygen-enriched porous capacitor carbon prepared in Example 1 is replaced by commercial activated carbon (YP-50F).

[0076] Performance Testing

[0077] Figure 1 This is a physical picture of the coal tar-based oxygen-rich porous capacitor carbon prepared in Example 1. Figure 1It can be seen that the coal tar-based oxygen-enriched porous capacitor carbon prepared by the present invention has a higher yield.

[0078] Figure 2 This is a SEM image of the coal tar-based oxygen-rich porous capacitor carbon prepared in Example 1. Figure 2 It can be seen that the coal tar-based oxygen-enriched porous capacitor carbon prepared in the present invention has a rich pore structure.

[0079] Figure 3 The coal tar-based oxygen-rich porous capacitor carbon (Y x CK) and the commercial activated carbon (YP-50F) of Comparative Example 1. Figure 3 It can be seen that the area enclosed by the cyclic voltammetry (CV) curve of the coal tar-based oxygen-enriched porous capacitor carbon prepared by the present invention is larger under the premise that the loading amount is 2.5 times that of the commercial activated carbon (YP-50F), and the coal tar-based oxygen-enriched porous capacitor carbon has a larger specific capacity.

[0080] Figure 4 The coal tar-based oxygen-rich porous capacitor carbon (Y x CK) and the constant current charge and discharge (GCD) diagram of the commercial activated carbon (YP-50F) of comparative example 1. Figure 4 It can be seen that the loading capacity of the coal tar-based oxygen-rich porous capacitor carbon prepared by the present invention is 2.5 times that of commercial activated carbon (YP-50F), and the discharge time is about 1 times that of commercial activated carbon (YP-50F), and the performance is much higher than that of commercial activated carbon (YP-50F).

[0081] Table 1 shows the test data of oxygen content, pore size, porosity and specific surface area of ​​the coal tar-based oxygen-enriched porous capacitor carbon and commercial activated carbon (YP-50F) prepared in Examples 1 to 7.

[0082] Table 1 Performance test results of coal tar-based oxygen-enriched porous capacitor carbon and commercial activated carbon (YP-50F) prepared in Examples 1 to 7

[0083] sample Oxygen content% Aperture nm <![CDATA[Porosity cm 3 / g]]> <![CDATA[Specific surface area m 2 / g <!-- 6 -->]]> Commercial activated carbon (YP-50F) - 0.8 0.7 1600 Example 1 15 0.6 0.9 2200 Example 2 12 0.6 0.6 2100 Example 3 23 1.2 1.2 2800 Example 4 18 2 1.5 2500 Example 5 14 2.8 0.5 2100 Example 6 10 1.8 0.8 2000 Example 7 20 1.5 1.1 2600

[0084] As can be seen from Table 1, the coal tar-based oxygen-enriched porous capacitor carbon prepared in the present invention has a larger oxygen content, porosity and specific surface area than commercial activated carbon (YP-50F).

[0085] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing coal tar-based oxygen-enriched porous capacitor carbon, characterized in that: The following steps are involved: The coal tar and the activator are mixed and pre-oxidized to obtain a pre-oxidized material; Carbonizing the pre-oxidized material at high temperature in a protective atmosphere to obtain coal tar-based oxygen-rich porous capacitor carbon; The activator includes one or more of alkaline earth metal hydroxides, alkaline earth metal carbonates, alkali metal hydroxides, alkali metal carbonates and alkali metal bicarbonates; The pre-oxidation is carried out in an atmosphere with an oxygen volume content of 5 to 20%; The temperature of the high temperature carbonization is 500-900°C.

2. The preparation method according to claim 1, characterized in that: The alkaline earth metal includes calcium and / or magnesium; the alkali metal includes potassium and / or sodium.

3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the coal tar to the activator is 1:0.5-4.

4. The preparation method according to claim 1, characterized in that: The pre-oxidation temperature is 150-450° C., and the heat preservation time is 0.5-3.5 hours.

5. The preparation method according to claim 1, characterized in that: The heat preservation time of the high temperature carbonization is 1 to 5 hours.

6. The preparation method according to claim 1 or 5, characterized in that: The protective atmosphere includes nitrogen, argon or helium; the flow rate of the protective atmosphere is 10 to 200 mL / min.

7. The preparation method according to claim 1, characterized in that: The heating rate to the high temperature carbonization temperature is 1 to 10° C. / min.

8. The preparation method according to claim 1, characterized in that: After the high-temperature carbonization, the method further includes: washing and drying the product of the high-temperature carbonization in sequence; the washing is acid leaching followed by washing with water until neutrality, or directly washing with water.

9. The coal tar-based oxygen-enriched porous capacitor carbon prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The coal tar-based oxygen-rich porous capacitor carbon has an oxygen mass percentage of 5-25%, a pore diameter of 0.5-20 nm, and a porosity of 0.5-2 cm 3 / g, specific surface area ≥2000m 2 / g.

10. Use of the coal tar-based oxygen-rich porous capacitor carbon according to claim 9 in supercapacitors.

Citation Information

Patent Citations

  • Method for preparation of activated carbon from carbon-rich residue of high temperature coal tar or coal tar pitch

    CN103204501A

  • Preparation method of two-dimensional porous carbon nanosheet for super capacitors

    CN105819419A

  • Porous graphene material and preparation method thereof, capacitor electrode, capacitor and electric device

    CN111039281A

  • Super capacitor carbon and preparation method thereof

    CN117985714A

  • Activated carbon for odor control and method for making same

    US20020082168A1