Porous calcium carbide coke pellet as well as preparation method and application thereof

By preparing porous calcium carbide coke pellets, using particle size adjustment of pulverized coal and calcium oxide powder and compound additives, the problem of low efficiency in the traditional calcium carbide industry has been solved, efficient and environmentally friendly calcium carbide production has been achieved, and resource waste and pollution have been reduced. .

CN118754126APending Publication Date: 2024-10-11李书军
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411013400.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The traditional calcium carbide industry is inefficient, and coke powder cannot be directly used in calcium carbide furnaces, resulting in resource waste and pollution. The lack of effective reduction technology results in coke powder can only be treated as low-grade fuel.

Method used

Porous calcium carbide coke pellets are used, prepared from coal powder, calcium oxide powder and composite additives. By adjusting the raw material particle size and process parameters, the reaction speed and efficiency are improved, and composite additives are used to enhance the thermal stability and stability of the pellets. active.

Benefits of technology

It significantly improves the output and production efficiency of calcium carbide, reduces electricity consumption, increases the molding rate and fixed carbon content of pellets without affecting its activity and specific resistance, and achieves efficient resource utilization and environmentally friendly production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of chemical engineering and environmental protection, and particularly relates to a porous calcium carbide coke pellet as well as a preparation method and application thereof. The porous calcium carbide coke pellet is prepared from the following raw materials in parts by weight: 60-70 parts of pulverized coal, 95-105 parts of calcium oxide powder and 1.5-2 parts of a compound additive. Through long-term research and exploration, the preparation raw material of the porous calcium carbide coke pellet can fully increase the specific surface area of the material, reduce the reaction activation energy and improve the production efficiency; and the adopted composite additive contains a large number of active groups and rich hole (porous) structures, so that the activity of the formed coke is not influenced, and relatively high specific resistance is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical industry and environmental protection, and specifically relates to a porous calcium carbide coke pellet and a preparation method and application thereof. Background Art

[0002] Coke and lignite are the main raw materials of calcium carbide chemical industry, occupying an important position in the national economy and playing a supporting role in enhancing the comprehensive national strength. While the total supply of coking coal and coke has decreased relatively, my country's annual crushed powder is more than 50 million tons. In the metallurgical, coal-to-gas chemical and other industries, coke is mostly used as a production raw material or fuel. The production has certain requirements on the particle size of coke blocks, so a lot of coke powder that cannot be directly used as production raw materials and fuel is screened out. Coke powder can only be used in small quantities as raw materials in cement plants and brick factories, making a large amount of coke powder useless.

[0003] The traditional calcium carbide industry mainly uses lump coal and lump quicklime as raw materials to produce calcium carbide, but this production method is inefficient, mainly due to the small contact area and slow reaction speed of lump coal and lump quicklime. With the increase of national environmental protection efforts, many small-scale coking enterprises have been closed, and the price of coke has continued to soar, and the coke powder and lignite powder produced cannot be directly used in calcium carbide furnaces. Coke powder has higher carbon content than coal-fired oil fixed carbon, lower volatility, and lower sulfur. Due to the lack of better reduction technology, a large amount of coke powder can only be processed as low-grade fuel. Therefore, using coke powder resources to become advantageous economic resources, preventing environmental pollution, accelerating the development of high-tech content, and increasing its added value have always been the topics explored by people in the coke powder deep processing industry.

[0004] Therefore, based on this, the technical solution of the present invention is proposed. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a porous calcium carbide coke pellet, which is prepared from the following raw materials in parts by weight: 60-70 parts of coal powder, 95-105 parts of calcium oxide powder and 1.5-2 parts of composite additives.

[0006] Preferably, the coal powder has fixed carbon ≥ 84wt.%, ash ≤ 8wt.%, volatile matter ≤ 8wt.%, and moisture < 1wt.%;

[0007] The particle size of the coal powder is 0.07-1 mm.

[0008] Preferably, in the calcium oxide powder, CaO ≥ 90 wt.%, MgO ≤ 1.8 wt.%, SiO 2 <2.5wt.%, raw, over-burned and impurities ≤15wt.%;

[0009] The particle size of the calcium oxide powder is 0.07-1 mm.

[0010] The inventors have conducted extensive research on the particle sizes of coal powder and calcium oxide powder, specifically:

[0011] During the exploration, it was found that the particle size of the raw materials, the gas flow rate during the preparation process, and the surface emissivity of the pellets all had an impact on the reaction results, and the degree of influence gradually decreased. When the particle size was reduced from 1mm to 0.71mm, the gas flow rate increased from 0.01m / s to 0.1m / s, and the surface emissivity increased from 0.7 to 0.9, the output of calcium carbide increased by 8.74%, 3.52% and 1.3% respectively in the same reaction time. Therefore, appropriate measures can be taken to enhance the heat transfer of the reaction layer. For example, the powder can be ground finer before pressing the mixed pellets, or the flue design of the calcium carbide furnace can be improved to reduce air resistance, thereby increasing the gas flow rate in the furnace. From the practical application point of view, it is obvious that grinding has a lower comprehensive cost than improving the flue design.

[0012] According to further research, when the contact area between coal powder and lime powder in the pellets is greatly increased, the chemical reaction rate will be accelerated and the energy consumption of the production process can be reduced. 2 The hourly output is 23389kg / h, the power consumption is 58057kWh, and the power consumption per kg of calcium carbide is only 2.48kWh / kg-CaC 2 , which is much lower than the average value of 3.26kWh / kg-CaC of traditional electric heating method. 2 Compared with the 3.26kWh / kg-CaC of the traditional electric heating method 2 Therefore, the particle size range of the raw materials selected by the present invention can fully increase the specific surface area of ​​the materials, reduce the reaction activation energy, and improve the production efficiency.

[0013] Preferably, the composite additive comprises sodium humate and a thickener; the mass ratio of the sodium humate to the thickener is 1:0.8-0.6; and the thickener is sodium carboxymethyl starch or dextrin.

[0014] The present invention has also conducted a lot of preliminary verifications on the composite additive. The composite additive of the present invention plays a bonding role and is the core of the coal powder and calcium oxide powder molding technology. It has been determined that the final molding rate is as high as 98%, the wet ball does not fall apart when dropped from a height of 2 meters, and can be dried naturally or by drying. After drying, the strength is 100 kg / ball, and the high temperature resistance is 900°C without falling or powdering. The composite additive does not contain chemical components such as magnesium, phosphorus, aluminum, and iron, and does not require heating and stirring of raw materials. The entire production process is pollution-free and suitable for small blast furnace ironmaking. It can replace part of the application of coke in industries such as metallurgical furnace materials, chemical coal gas raw materials, and calcium carbide production raw materials. This advantage cannot be ignored.

[0015] The thermal stability of the additive that plays a bonding role is very important. The temperature measurement point requirement for thermal stability of porous calcium carbide coke pellets is more than 200°C higher than that of briquette coal. Most existing organic adhesives have collapsed when the coke reaches 900°C. Although some inorganic adhesives can ensure thermal stability, the addition amount is more than 10%. The higher additive amount causes the fixed carbon of the pellets to drop seriously, making them unusable. The amount of the composite additive described in the present invention can ensure the thermal stability of the pellets without reducing the fixed carbon of the pellets.

[0016] In addition, the additives should also ensure the activity of the pellets. The production of calcium carbide requires the carbon raw materials to have higher activity, and the adhesive used in the present invention contains a large number of active groups and rich pore (porous) structures, which can ensure that the activity of the coke is not affected and maintain a higher resistivity.

[0017] The composite additive of the present invention contains both inorganic compounds that can withstand high temperatures and organic polymer compounds with good bonding properties, which fundamentally changes the defects of a single binder. The additive has the advantages of good mutual solubility, strong bonding force, easy solvent volatility, high compressive strength of coke particles after drying, high temperature resistance, good chemical reaction activity, abundant raw material sources, simple molding process and low comprehensive molding cost, and is an ideal additive for calcified coke pellets.

[0018] Based on the same technical concept, the present invention further provides a method for preparing porous calcium carbide coke pellets, the preparation method comprising the following steps:

[0019] (1) Coal powder and calcium oxide powder are fully mixed, and water and a composite additive are added, and the mixture is stirred evenly to obtain a mixed raw material;

[0020] (2) pelletizing the mixed raw material to obtain ellipsoidal pellets;

[0021] (3) drying the ellipsoidal pellets to obtain dried pellets;

[0022] (4) The dried pellets are cooled and screened in sequence to obtain the finished porous calcium carbide coke pellets.

[0023] Preferably, in step (1), the mass of water added is 10 to 20 wt.% of the total mass; and the stirring time is 30 to 40 minutes.

[0024] Preferably, in step (2), the pressure of the ball pressing process is 250 kgf / cm 2 .

[0025] In the process of pressing balls, when the pressure is too low, the green balls are easy to break, difficult to transport, and the initial strength is not good. If too high a pressure is used, although the initial strength of the green balls is enhanced, the porosity between the internal particles of the over-dense balls decreases, resulting in a decrease in gasification rate, a decrease in reaction activity, a prolonged gasification time, and an increase in residual carbon. It is also very important to select a suitable pressure. Therefore, the pressure used in the present invention is 250kgf / cm 2 .

[0026] The shapes of pellets are generally square pillow and ellipsoid. From the perspective of mold release, the ellipsoid is easier to demold than the square pillow. At the same time, the ellipsoid has good thermal fission properties and is easy to burn completely. The pellets we choose are ellipsoidal, with a size of 40mm×35mm×25mm (long axis×short axis×height) to improve the utilization rate of fixed carbon in the pellets.

[0027] Preferably, in step (3), the drying is divided into three stages; wherein:

[0028] The temperature of the first stage is 255-265°C or 275-285°C;

[0029] The temperature of the second stage is 285-295°C;

[0030] The temperature of the third stage is 120-200°C.

[0031] More specifically, in the first stage, the pellets are preheated to a certain temperature to prepare for the next drying stage. When the moisture content of the pellets is ≤20%, the hot air temperature in this area is controlled at 255-265°C; when the moisture content is ≥20%, the hot air temperature in this area is controlled at 275-285°C.

[0032] In the second stage, the temperature is 285-295℃, during which the coal powder and calcium oxide powder undergo pyrolysis reaction to generate carbonaceous substances and form porous calcium carbide coke pellets. The purpose of this stage is to reduce the moisture content in the pellets and increase the carbonization rate and mechanical strength.

[0033] In the third stage, the temperature is 120-200°C, and the pellets are finally dried.

[0034] In subsequent operations, the dried pellets are naturally cooled to reduce their temperature to an appropriate level, and then the cooled pellets are screened to remove unqualified pellets (the purpose of screening is to obtain calcified coke pellet products that meet the requirements). Finally, the qualified calcified coke pellets are stored, or they can be directly hot-loaded and hot-delivered into the calcium carbide furnace (moisture content <1%) to better reduce the calcium carbide reaction time.

[0035] Based on the same technical concept, the solution of the present invention is to provide another application of porous calcium carbide coke pellets in the preparation of calcium carbide.

[0036] The beneficial effects of the present invention are:

[0037] After long-term research and exploration, the raw materials for preparing the porous calcium carbide coke pellets of the present invention can fully increase the specific surface area of ​​the material, reduce the reaction activation energy, and improve production efficiency; and the composite additives used in the present invention contain a large number of active groups and rich cavities (porous) structures, which can ensure that the activity of the coke is not affected and maintain a high specific resistivity. DETAILED DESCRIPTION

[0038] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0039] Example 1

[0040] This embodiment provides a method for preparing porous calcium carbide coke pellets, the preparation method comprising the following steps:

[0041] (1) 65 kg of coal powder and 100 kg of calcium oxide powder are fully mixed to ensure the uniformity of the raw materials and prepare for the subsequent pelletizing process, and water (accounting for 15 wt.% of the total amount) and a composite additive (1 kg of sodium humate and 0.8 kg of carboxymethyl starch) are added, and the mixture is stirred in a mixer for 35 minutes and then aged to obtain a mixed raw material;

[0042] (2) The mixed raw material is pelletized at a pressure of 250 kgf / cm 2 , and obtain ellipsoidal spheroids;

[0043] (3) drying the ellipsoidal pellets at 260° C. for the first stage, then drying them at 290° C. for the second stage, and finally drying them at 160° C. for the third stage (drying) to obtain dried pellets;

[0044] (4) The dried pellets are cooled and screened in sequence to remove unqualified pellets, thereby obtaining the finished porous calcium carbide coke pellets.

[0045] Example 2

[0046] This embodiment provides a method for preparing porous calcium carbide coke pellets, the preparation method comprising the following steps:

[0047] (1) 60 kg of coal powder and 95 kg of calcium oxide powder are fully mixed to ensure the uniformity of the raw materials and prepare for the subsequent pelletizing process, and water (accounting for 10 wt.% of the total amount) and a composite additive (1 kg of sodium humate and 0.6 kg of dextrin) are added, and the mixture is stirred in a mixer for 30 minutes and then aged to obtain a mixed raw material;

[0048] (2) The mixed raw material is pelletized at a pressure of 250 kgf / cm 2 , and obtain ellipsoidal pellets;

[0049] (3) drying the ellipsoidal pellets at 255° C. for the first stage, then drying them at 285° C. for the second stage, and finally drying them at 120° C. for the third stage (drying) to obtain dried pellets;

[0050] (4) The dried pellets are cooled and screened in sequence to remove unqualified pellets, thereby obtaining the finished porous calcium carbide coke pellets.

[0051] Example 3

[0052] This embodiment provides a method for preparing porous calcium carbide coke pellets, the preparation method comprising the following steps:

[0053] (1) 70 kg of coal powder and 105 kg of calcium oxide powder were fully mixed to ensure the uniformity of the raw materials and prepare for the subsequent pelletizing process, and water (accounting for 20 wt.% of the total amount) and a composite additive (1 kg of sodium humate and 0.6 kg of dextrin) were added, and the mixture was stirred in a mixer for 30 minutes and then aged to obtain a mixed raw material;

[0054] (2) The mixed raw material is pelletized at a pressure of 250 kgf / cm 2 , and obtain ellipsoidal spheroids;

[0055] (3) drying the ellipsoidal pellets at 280° C. for the first stage, then drying them at 295° C. for the second stage, and finally drying them at 200° C. for the third stage (drying) to obtain dried pellets;

[0056] (4) The dried pellets are cooled and screened in sequence to remove unqualified pellets, thereby obtaining the finished porous calcium carbide coke pellets.

[0057] Verification Example

[0058] The indicators of the porous calcium carbide coke pellets obtained in Example 1 of the present invention are shown in Table 1.

[0059] Table 1

[0060] name Porous calcium carbide coke pellets index Appearance and structure Ellipsoid color light black size Length 40mm Width 35mm Thickness 25mm Ash content (mass percentage) ≤10% Fixed carbon (mass percentage) ≥80% Cold Strength ≥400N / pc Thermal Strength ≥300N / pc

[0061] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A porous calcium carbide coke pellet, characterized in that: The invention is prepared from the following raw materials in parts by weight: 60-70 parts of coal powder, 95-105 parts of calcium oxide powder and 1.5-2 parts of composite additive.

2. The porous calcium carbide coke pellet according to claim 1, characterized in that: The coal powder has a fixed carbon content of ≥84wt.%, an ash content of ≤8wt.%, a volatile matter content of ≤8wt.%, and a moisture content of <1wt.%; The particle size of the coal powder is 0.07-1 mm.

3. The porous calcium carbide coke pellet according to claim 1, characterized in that: The calcium oxide powder contains CaO ≥ 90 wt.%, MgO ≤ 1.8 wt.%, SiO2 < 2.5 wt.%, and raw, over-burned and impurities ≤ 15 wt.%; The particle size of the calcium oxide powder is 0.07-1 mm.

4. The porous calcium carbide coke pellets according to claim 1, characterized in that: The composite additive comprises sodium humate and a thickener; the mass ratio of the sodium humate to the thickener is 1:0.8-0.6; and the thickener is sodium carboxymethyl starch or dextrin.

5. The method for preparing porous calcium carbide coke pellets according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) Coal powder and calcium oxide powder are fully mixed, and water and a composite additive are added, and the mixture is stirred evenly to obtain a mixed raw material; (2) pelletizing the mixed raw material to obtain ellipsoidal pellets; (3) drying the ellipsoidal pellets to obtain dried pellets; (4) The dried pellets are cooled and screened in sequence to obtain the finished porous calcium carbide coke pellets.

6. The method for preparing porous calcium carbide coke pellets according to claim 5, characterized in that: In step (1), the mass of water added is 10 to 20 wt.% of the total mass; and the stirring time is 30 to 40 minutes.

7. The method for preparing porous calcium carbide coke pellets according to claim 5, characterized in that: In step (2), the pressure of the ball pressing process is 250kgf / cm 2 .

8. The method for preparing porous calcium carbide coke pellets according to claim 5, characterized in that: In step (3), the drying is divided into three stages; wherein: The temperature of the first stage is 255-265°C or 275-285°C; The temperature of the second stage is 285-295°C; The temperature of the third stage is 120-200°C.

9. Use of the porous calcium carbide coke pellets according to any one of claims 1 to 4 in the preparation of calcium carbide.

Citation Information

Patent Citations

  • Method of preparing pellet for producing calcium carbide

    CN107572527A

  • Preparation method of high-performance pellets and application of high-performance pellets in pellet sintering process

    CN114540616A

  • Calcium carbide production method and production system

    CN116443879A

  • Method for preparing calcium carbide by using plasma pyrolysis technology and prepared calcium carbide

    CN118343760A

  • Method for generating calcium carbide using electrothermal method

    WO2020087633A1