A catalyst support, macroporous silica gel, and its preparation method
By using the synergistic effect of pH indicator and template agent in the preparation of macroporous silica gel, the problem of difficulty in controlling the gel reaction node is solved, achieving efficient preparation of macroporous silica gel, increasing pore volume and specific surface area, reducing cost, and making it suitable for catalyst supports.
Patent Information
- Application Number
- CN202410768393.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The current macroporous silica gel preparation process suffers from difficulties in controlling the primary gel point, uneven pore size distribution, high cost, and difficulty in precise control, which affects catalytic performance.
By using the synergistic effect of pH indicator and template agent, the gel reaction node is determined by color change. Combined with hydrolysis and acid washing steps, macroporous silica gel is prepared. Polyethylene glycol in the dyeing waste liquid is used as template agent and dispersant to control the formation of gel micronuclei and pore expansion.
It achieves sensitive and accurate control of the gelation reaction, reduces production costs, increases the pore volume and specific surface area of macroporous silica, enhances the skeleton strength, and is suitable for polyolefin catalyst supports.
Smart Images

Figure BDA0004893312860000081 
Figure BDA0004893312860000082 
Figure BDA0004893312860000091
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic materials technology, and in particular to a catalyst support macroporous silica gel and its preparation method. Background Technology
[0002] Silica gel is primarily used in the petrochemical industry as a catalyst and catalyst support, playing a crucial role in catalyst components. The internal pore structure of silica gel has a significant impact on the morphology of polymers. Currently, most of the silica gel used as catalyst supports in the polyolefin industry relies on imports, making domestic substitution imperative.
[0003] Existing methods for preparing macroporous silica gel mainly involve adjusting the addition method and reaction conditions of silicates and acids to induce a reaction between the silicates and acids. However, these methods have the following problems: the primary gel contains a large number of small pores, resulting in a wide pore size distribution that affects catalytic performance. For example, patent application number CN200610129489.8 describes the production of macroporous silica gel support for ethylene polymerization catalysts by reacting water glass with inorganic acids in a certain ratio under pH conditions of 2-4. Secondly, existing methods for preparing macroporous silica carriers suffer from the problem that the primary gel point appears quickly and is difficult to control, hindering the dispersion of the primary gel. For example, patent CN102745698 B discloses a method for preparing a silica carrier. This method involves adding a silicate solution and reacting it with an inorganic acid at pH 2-4 to form a primary gel, followed by secondary and tertiary gel formation at pH 7-9 and pH 10-12. Macroporous silica carriers are prepared through repeated gelation. However, in this method, the initial gelation point of the macroporous silica appears quickly and is difficult to control, making it hard to accurately determine the key points of the gelation reaction. Furthermore, the preparation cost of the aforementioned macroporous silica is relatively high. Therefore, the existing technology needs further improvement. Summary of the Invention
[0004] To address the aforementioned issues, this invention provides a method for preparing macroporous silica gel catalyst support that is easier to control in terms of coagulation point, simpler to operate, and lower in cost, as well as the prepared product. It prepares macroporous silica gel catalyst support through the gel micro-nucleus indication effect of pH indicator liquid and the pore-expanding effect of template agent.
[0005] To address the above problems, the present invention provides the following technical solution:
[0006] A method for preparing macroporous silica gel carrier, comprising the following steps:
[0007] S1. Add pH indicator solution and template agent to inorganic acid, stir evenly, and then keep at a constant temperature for 1 to 3 hours. The solution will show the first color.
[0008] S2. Add silicate solution. When the color of the system changes, primary micronuclei are formed. Add more than 3 times the amount of water to disperse the primary micronuclei quickly.
[0009] S3. Continue adding silicate solution. Stop adding when the system color changes again. Stir at a constant temperature until homogeneous, then add acid until the system color changes again, thereby stabilizing the particle skeleton.
[0010] S4. The system is then subjected to acid washing, water washing, pulping, spray drying, and high-temperature calcination in sequence to obtain the carrier macroporous silica gel.
[0011] Preferably, in step S2, a silicate solution with a weight percentage concentration of 8-25% based on silica content is added. When the system color changes, primary micronuclei are formed. Then, 3-8 times the amount of water is added to rapidly disperse the primary micronuclei.
[0012] In the above scheme, the raw materials for preparing silica gel are silicate solution, template agent solution and acid solution. Since a pH indicator solution is added to the system, the solution changes color as the pH changes during the reaction. By capturing the color change of the system, the next step is initiated, allowing the raw materials to gradually react with each other to form a gel skeleton.
[0013] The reaction principle is as follows: ① Silicates undergo hydrolysis in acidic aqueous solutions. Based on the ionization equilibrium constant and pH stability range of silicic acid, silicic acid is stable in the pH range of 2-3. When pH > 4, monosilicic acid begins to condense into nuclei. The color change point of the selected indicator coincides with the hydrolysis and condensation point of silicates. The arrival of the change point is quickly determined based on the color change of the indicator (around pH 4), and sufficient water is added to the system in time to rapidly disperse the primary micronuclei; ② Then, silicates are added to the system until the solution color changes again (around pH 10). During this process, the silicates in the system continue to hydrolyze, forming connecting bridges between local micronuclei, connecting the dispersed micronuclei into a cage-like loose porous structure; ③ Then, an acid solution is added to the system and kept at a constant temperature for several hours. The acid treatment makes the gel skeleton more stable. Then, acid is added to the system until the system color changes again (pH=3), and then the addition is stopped. The excess acid replaces the salt in the skeleton, completing the acid washing, which facilitates the subsequent water washing; ④ The formed gel is then washed with water, dried and calcined at high temperature to obtain a macroporous powdered silica gel product.
[0014] The final macroporous silica gel has a silica content of over 99% and a specific surface area >300m². 2 / g, pore volume > 1.55cm 3 / g, and the load breakage rate is less than 10%, and the skeleton strength is significantly improved.
[0015] Compared to existing methods for detecting pH in macroporous silica gel preparation by inserting a pH meter electrode probe into the reaction system, which suffers from slow reaction detection and insufficient sensitivity, and can also affect the accurate identification of critical reaction points due to silica condensation and clogging of the pH electrode probe, this application introduces a pH indicator solution into the system. This solution offers advantages such as rapid and sensitive detection, as well as high accuracy, thus solving the aforementioned problems of the existing technology. Furthermore, this method allows for timely detection of primary micronuclei formation, preventing the formation of a gel-like structure due to delayed water dispersion, which hinders subsequent reactions and results in a silica gel product with a small pore volume and specific surface area.
[0016] Furthermore, and more importantly, the pH indicator solution preferred in this application contains polyethylene glycol at a weight percentage concentration of 5-15%. For example, dyeing waste liquid containing polyethylene glycol surfactants (weight percentage concentration of 5-15%) can be used directly. On the one hand, this method can recycle and utilize the dyeing waste liquid in the production of pH color-changing indicator silica gel (such as the patent application number 202210936482.6, "A pH color-changing indicator silica gel"), reducing raw material costs. On the other hand, the polyethylene glycol in the dyeing waste liquid can not only disperse the gel micronuclei, but also act as a template agent to expand pores. During the gelation process, the polyethylene glycol is encapsulated in the skeleton, and the pores are generated after removal by calcination.
[0017] Preferably, in the above method for preparing macroporous silica gel, the pH indicator solution is selected from one, two, or more of the following: quinalidine red, bromothymol blue, phenolphthalein, thymol blue, bromophenol blue, methyl red, methyl orange, dimethyl yellow, catechol purple, Nell blue, ethoxyflavin, naphthol, and m-cresol purple. Preferably, the pH indicator solution is selected from methyl red, quinalidine red, bromothymol blue, catechol purple, and phenolphthalein.
[0018] The pH indicator solution uses a combination of one or more indicators, whose color change point corresponds to the silicate hydrolysis and condensation point and other key nodes in the two-step skeleton synthesis. The color change of the indicator helps operators accurately grasp the operational nodes of each step. Optionally, the pH indicator solution is a mixture of methyl red and bromothymol blue, a mixture of methyl red and phenolphthalein, or a mixture of quinalidine red and catechol purple.
[0019] Preferably, in the method for preparing the macroporous silica gel carrier, the acid is selected from one of hydrochloric acid, sulfuric acid, nitric acid, citric acid, acetic acid, and oxalic acid; preferably, hydrochloric acid or sulfuric acid is used.
[0020] Preferably, in the method for preparing the macroporous silica gel carrier, the template agent is selected from one or two of ammonium bicarbonate, ammonium carbonate, ammonia, ammonium bisulfate, ammonium chloride, and ammonium acetate; preferably, the template agent is ammonia or ammonium bisulfate.
[0021] Preferably, in the method for preparing the macroporous silica gel carrier, the silicate is selected from one or more of sodium silicate, potassium silicate, and lithium silicate. More preferably, the silicate is sodium silicate.
[0022] More preferably, step S1 involves adding a pH indicator solution (final concentration of 0.5-2‰) to 200-1000 mL of an inorganic acid with a mass percentage concentration of 5-20%, adding a template agent (final concentration of 5-15%) at 15-60°C, and treating at a constant temperature for 1-2 hours.
[0023] Preferably, step S2 involves maintaining the temperature at 45–60°C, then adding a silicate solution with a mass percentage concentration of 8–25% based on silica content. When the system color changes, primary micronuclei are formed. Then, 3–8 times the amount of water is added to rapidly disperse the primary micronuclei.
[0024] Preferably, step S3 involves continuing to add a silicate solution with a mass percentage concentration of 8-25% based on the silica content. Once the system color changes again, the addition is stopped. After stirring at a constant temperature for 1-3 hours, an inorganic acid with a mass percentage concentration of 5-10% is added, and the mixture is kept at this temperature for 5-10 hours, thereby promoting the stability of the particle skeleton.
[0025] Preferably, step S4 involves adding acid (1-5% by mass) to the system until the system color changes again, followed by acid washing; then washing with water at 50-70°C; adding 0.5%-10% by mass of binder to form a slurry and spray drying at 200-300°C; and finally calcining at 750-850°C for 0.5-1.5 hours.
[0026] The binder can be one or more of silica sol, potassium silicate, or sodium silicate. Preferably, the amount of silica sol added is 4%-10%, the amount of potassium silicate added is 0.5-6%, and the amount of sodium silicate added is 0.3-5% (all by mass percentage). The function of adding the binder is to form a film on the particle surface, increase the surface strength of the particles, and make the particle skeleton stronger after spray molding.
[0027] Preferably, the calcination conditions are 800°C for 1 hour. Compared to the gradient heating in this stage of the prior art, this treatment, combined with the aforementioned treatment, is more conducive to improving the overall framework strength of the macroporous silica gel supported catalyst.
[0028] The method for preparing the carrier macroporous silica gel of the present invention has the following beneficial effects:
[0029] 1. The method for preparing macroporous silica gel provided by this invention can promptly determine the formation of primary micronuclei and other important nodes through the gel micronucleus indication effect of pH indicator liquid and the pore-expanding effect of template agent. It has the advantages of sensitive, fast and accurate detection. The prepared silica gel has large pore volume and large specific surface area, and can be used as a support for polyolefin catalysts. It has good application prospects as a catalyst support.
[0030] 2. The method for preparing macroporous silica gel of the present invention can directly use dyeing waste liquid mixed with polyethylene glycol surfactants as pH indicator liquid, which can not only greatly reduce production costs, but also reduce environmental pollution and resource waste. In addition, the polyethylene glycol mixed in the dyeing waste liquid can not only play the role of dispersing gel micronuclei, but also play a certain role of pore expansion as a template agent, further improving the comprehensive performance of silica gel products, such as increasing pore volume and specific surface area. Detailed Implementation
[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. In the present invention, unless otherwise specified, the equipment and raw materials used can be purchased from the market or are commonly used in the art. Unless otherwise specified, the methods in the following embodiments are conventional methods in the art.
[0032] Example 1
[0033] (1) Pour 200 mL of 16% dilute sulfuric acid solution into the reaction vessel, add 30 mL of methyl red and bromothymol blue mixed indicator (containing 5% polyethylene glycol), turn on the stirrer, add 30 mL of 8% ammonia solution at 35°C, and keep the temperature constant for 1.5 h after the addition is complete. The solution turns red.
[0034] (2) After heating to 50℃, add a 14% sodium silicate solution; when the solution changes from red to yellow and gel micronuclei appear, add 800mL of distilled water to disperse the gel micronuclei evenly.
[0035] (3) Continue adding sodium silicate solution until the solution turns dark blue, stop adding and keep the temperature constant for 1.5 h; then add 100 ml of 6% dilute sulfuric acid to stabilize the gel skeleton, keep the temperature constant for 10 h and then add 500 ml of 3% dilute sulfuric acid solution to acidify until it turns yellow-green.
[0036] (4) After washing with water at 50°C, add 10g of 30% silica sol to make a slurry, spray dry at 220°C, and then calcine at 800°C for 1 hour to obtain macroporous powdered silica gel product.
[0037] The product performance is shown in Table 1.
[0038] Example 2
[0039] (1) Place 400 mL of 20% dilute hydrochloric acid solution in a reaction vessel, add 0.785‰ methyl red and phenolphthalein mixed indicator (containing 3% polyethylene glycol), turn on the stirrer, add 50 mL of 15% ammonium bisulfate aqueous solution at 60℃, and keep the temperature constant for 1 h.
[0040] (2) Add a 24% sodium silicate solution; when the solution changes from red to orange and gel micronuclei appear, quickly add 2000 mL of distilled water to disperse the micronuclei evenly.
[0041] (3) Continue adding sodium silicate solution until the solution turns dark red, stop adding and keep the temperature constant for 3 hours; then add 200 ml of 7% dilute hydrochloric acid to stabilize the gel skeleton, keep the temperature constant for 5 hours and then add 200 ml of 5% dilute hydrochloric acid solution to acidify until yellow.
[0042] (4) After washing with water at 70°C, add 5g of 30% potassium silicate and slurry. After spray drying at 300°C, calcine at 800°C for 1 hour to obtain macroporous powdered silica gel product.
[0043] The product performance is shown in Table 1.
[0044] Example 3
[0045] (1) Place 1000 mL of 5% dilute sulfuric acid solution in a reaction vessel, add quinacrine red and catechol purple indicator (containing 5% polyethylene glycol), turn on the stirrer, slowly add 300 mL of 5% ammonium bisulfate solution at 15°C, and after 1.5 h at a constant temperature, the solution becomes colorless.
[0046] (2) Heat to 50℃ and add 8% sodium silicate solution; when the solution changes from colorless to red and gel micronuclei appear, add 5000mL of distilled water to disperse the gel micronuclei.
[0047] (3) Continue adding sodium silicate solution until the solution turns purple-red, stop adding and keep the temperature constant for 1.5 hours, then add 200 ml of 6% dilute sulfuric acid to promote continued gelation;
[0048] (4) Finally, heat the temperature to 60°C, keep it at the temperature for 7 hours, add dilute sulfuric acid solution to acidify until yellow; wash with water at 50°C, add 13g of 30% sodium silicate to pulp, spray dry at 220°C, and calcine at 800°C for 1 hour to obtain the silica gel product.
[0049] The product performance is shown in Table 1.
[0050] Comparative Example 1
[0051] Macroporous silica gel was prepared according to the scheme of Example 1 of existing patent CN102745698 B:
[0052] Place 200 ml of a 1.1 mol / L dilute sulfuric acid solution in a reaction vessel, turn on the stirrer, and slowly add 30 ml of a 5.0 mol / L ammonia solution at 30°C. After the addition is complete, maintain the temperature for 1 hour. Raise the temperature to 50°C and add a 1.3 mol / L sodium silicate solution at a rate of 3.0 ml / min. When the initial gelation of the solution is complete, quickly add 400 ml of distilled water and stir to completely disperse the silica gel. Continue adding sodium silicate solution until the pH of the solution reaches 11 (measured with a pH meter). Stop adding sulfuric acid and maintain the temperature for 1 hour; add 1.1 mol / L dilute sulfuric acid solution at a rate of 4.0 ml / min to promote further gelation of the silica gel. When the pH of the solution reaches 9 (measured with a pH meter), stop adding dilute sulfuric acid and maintain the temperature for 1 hour; finally, raise the temperature to 70℃, maintain the temperature for 5 hours, and then quickly add dilute sulfuric acid solution for acidification. Then wash and pulp with distilled water, spray dry at 220℃, and activate using a gradient temperature increase (200℃ (1 hour) - 400℃ (1 hour) - 600℃ (2 hours)) to obtain the silica gel product. The performance of the product is shown in Table 1.
[0053] Comparative Example 2
[0054] Except for the absence of polyethylene glycol in the preparation process, the preparation process is the same as in Example 1. The performance of the product is shown in Table 1.
[0055] Comparative Example 3
[0056] Except for the absence of a pH indicator solution containing polyethylene glycol during preparation, the preparation process is the same as in Example 1. The performance of the product is shown in Table 1.
[0057] Silicone Performance Test Examples
[0058] The silicone products prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to various performance tests according to the following methods.
[0059] 1. Method for determining the pore volume of silica gel – water titration method
[0060] Weigh 10g of the sample, dried at (150±5)℃, accurate to 0.01g. Place it in a dry 250mL Erlenmeyer flask with a ground glass stopper. Accurately add approximately 5mL of water at a time using a 25mL burette. Seal the flask and shake it for 5 minutes until the sample becomes loose. Then, open the stopper and add water dropwise, shaking the flask after each addition. If the sample remains loose after shaking, continue adding water dropwise. The titration endpoint is reached when the sample particles begin to adhere to each other and the flask wall, and this adhesion persists after shaking for 1 minute. Record the volume of water consumed.
[0061] The pore volume w8, expressed in mL / g, is calculated according to formula (1):
[0062]
[0063] In the formula:
[0064] V – The numerical value of the volume of water consumed, in milliliters (mL).
[0065] m — the numerical value of the sample mass, in grams (g).
[0066] The arithmetic mean of the parallel determination results is taken as the determination result, and the absolute difference between two parallel determination results is not greater than 0.02 mL / g.
[0067] 2. Method for determining the specific surface area of silica gel – BET method
[0068] Weigh 0.2g–0.3g of the dried sample to constant mass, accurate to 0.0002g. Place it in the measuring tube and degas under vacuum at 150℃–200℃ for 2 hours until the vacuum level reaches below 1 Pa. Begin measuring the adsorption isotherm. Dead volume correction needs to be initiated for the first measurement. BET equation:
[0069] P / V(Po-P)=1 / VmC+[(C-1) / VmC](P / Po)
[0070] Analysis indicates that in the range of (P / Po) 0.05-0.35, the BET equation is a linear equation. The reciprocal of the sum of the slope and intercept of this line is exactly the monolayer saturated adsorption capacity. Therefore, within this range, by selecting 3-5 pressure points, measuring the adsorption capacity at each pressure point, and then plotting according to the BET equation, the monolayer saturated adsorption capacity can be obtained, and the specific surface area can be calculated.
[0071] 3. Average pore size of silicone Measurement methods
[0072] The calculation for silica gel pore size is: pore size = 40000 * pore volume / specific surface area.
[0073] 4. Method for determining the skeleton strength (load breakage rate) of silicone rubber
[0074] The method for testing the skeleton strength involves adding silicone to an organic solvent, stirring at high temperature for 8 hours, drying, and then observing and comparing the breakage under a microscope.
[0075] Table 1. Performance comparison of macroporous silica gel in each embodiment.
[0076]
[0077]
[0078] According to the experimental results in Table 1 above, compared with the existing scheme of Comparative Example 1, the average pore size of the macroporous silica gel prepared in Examples 1 to 3 of this application is improved and the skeleton strength is significantly improved. In particular, the pore volume and specific surface area of the macroporous silica gel in Example 1 are significantly better than those in Comparative Example 1.
[0079] Compared to Comparative Example 3, Example 1 showed a significant reduction in pore volume, specific surface area, and average pore size. This indicates that using a pH indicator solution containing polyethylene glycol helps to accurately determine the formation of primary micronuclei and other important nodes, thus greatly improving the quality of macroporous silica gel.
[0080] It is understood that those skilled in the art can make equivalent substitutions or modifications to the technical solutions and concepts of this invention, and all such substitutions or modifications should fall within the protection scope of the appended claims.
Claims
1. A method for preparing macroporous silica gel as a catalyst support, characterized in that, Includes the following steps: S1. Add pH indicator solution and template agent to inorganic acid, stir evenly, and the solution will show the first color; the pH indicator solution contains polyethylene glycol with a weight percentage concentration of 5-15%; S2. Add a silicate solution with a weight percentage concentration of 8-25% based on silica content. When the system color changes, primary micronuclei are formed. Add 3-8 times the amount of water to quickly disperse the primary micronuclei. S3. Continue adding silicate solution. Stop adding when the color of the system changes again. Stir at a constant temperature until homogeneous, then add acid to stabilize the particle skeleton. S4. The system is then subjected to acid washing, water washing, pulping, spray drying, and high-temperature calcination in sequence to obtain the carrier macroporous silica gel.
2. The method for preparing macroporous silica gel catalyst support according to claim 1, characterized in that, The acid is selected from one of the following: hydrochloric acid, sulfuric acid, nitric acid, citric acid, acetic acid, and oxalic acid. The silicate is selected from one or more of sodium silicate, potassium silicate, and lithium silicate.
3. The method for preparing macroporous silica gel catalyst support according to claim 2, characterized in that, The acid is selected from hydrochloric acid or sulfuric acid.
4. The method for preparing macroporous silica gel catalyst support according to claim 2, characterized in that, The silicate is selected from sodium silicate.
5. The method for preparing macroporous silica gel catalyst support according to claim 1, characterized in that, The template agent is selected from one or two of ammonium bicarbonate, ammonium carbonate, ammonia, ammonium bisulfate, ammonium chloride, and ammonium acetate.
6. The method for preparing macroporous silica gel catalyst support according to claim 5, characterized in that, The template agent is selected from ammonia or ammonium bisulfate.
7. The method for preparing macroporous silica gel catalyst support according to claim 1, characterized in that, The pH indicator solution is selected from one, two or more of the following: quinaldinine red, bromothymol blue, phenolphthalein, thymol blue, bromophenol blue, methyl red, methyl orange, dimethyl yellow, catechol purple, Nyl blue, ethoxyflavin, naphthol, and m-cresol purple.
8. The method for preparing macroporous silica gel carrier according to claim 1, characterized in that, Step S1 involves adding a pH indicator solution to 200-1000 mL of an inorganic acid with a mass percentage concentration of 5-20%, adding a template agent at 15-60°C, and maintaining the temperature for 1-2 hours.
9. The method for preparing macroporous silica gel catalyst support according to claim 1, characterized in that, Step S2 involves maintaining the temperature at 45-60℃, then adding a silicate solution with a mass percentage concentration of 8-25% based on silica content. When the system color changes, primary micronuclei are formed. Add 3-8 times the amount of water to rapidly disperse the primary micronuclei.
10. The method for preparing macroporous silica gel catalyst support according to claim 1, characterized in that, Step S4 involves adding acid to the system until the system color changes again, followed by acid washing; then washing with water at 50-70°C, adding binder for pulping, and spray drying at 200-300°C, followed by calcination at 750-850°C for 0.5-1.5 hours.
Citation Information
Patent Citations
Preparation method of carrier silica gel
CN102745698B
A pH color-changing indicating silica gel and preparation method thereof
CN115219490B
Method for preparing macroporous silicon rubber carrier for ethylene polymerization catalyst by vapour process
CN1978470A
Preparation method of carrier silica gel
CN102745698A
Nano-silicon dioxide used for nanometer standard granule