Method for preparing hectorite through water vapor crystallization
The direct preparation of hectorite through the water vapor crystallization method solves the high cost, low output and complex process problems of hectorite production in the hydrothermal method, and achieves the effects of high solid content and simplified process.
Patent Information
- Application Number
- CN202410906281.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing hydrothermal method for preparing laponite has the problems of high cost, low yield, complex process, difficulty in treating wastewater and difficulty in filtration.
Using the water vapor crystallization method, hectorite is directly prepared by reacting lithium salt, magnesium salt and water glass under specific conditions to form a gel, and then crystallizing it in high temperature and high pressure water vapor, which solves the problem of low solid content and filtration. Difficult and complex issues of wastewater treatment.
It achieves the preparation of hectorite with high solid content, simplifies the process, reduces drying costs, solves the complexity and filtration problems of wastewater treatment in hydrothermal methods, and improves production efficiency.
Smart Images

Figure CN118754144A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laponite preparation, and in particular to a method for preparing laponite by water vapor crystallization. Background Art
[0002] Hectorite is a 2:1 layered clay mineral material with a molecular structure of M x [Li x Mg 6-x Si 8 O 20 (OH·F) 4 ](M=Na, Li). In the vertical direction, Si-O tetrahedrons and Mg-O octahedrons are arranged in an orderly manner in a ratio of 2:1. The average layer thickness of the layer is about 1nm and the diameter is about 30nm. 2+ Li + Substitution, negatively charged, so the interlayer adsorption of Li + Or Na + Equal cations to balance the charge.
[0003] When laponite is dispersed in water, the interlayer adsorbed cations of the lamellar structure undergo hydration, the volume increases, and the exfoliation dissolution occurs, forming thin flake particles with a thickness of about 1nm and a diameter of about 30nm. The surface of this flake carries a certain amount of negative charge, while the Mg-OH at the edge will be protonated and carry a certain amount of positive charge, such as Figure 1 The negative charges on the surface of the sheet and the positive charges on the edge of the sheet attract each other, forming a continuous network structure, which is figuratively called a "card house" structure, as shown in Figure 2 As shown. This "card house" structure remains stable under static conditions, but when a certain external force is applied, this network structure will be destroyed. However, when the external force stops, this stable "card house" structure will be re-formed. This is the thixotropy of lithium soapstone in water. It is precisely because lithium soapstone has good swelling, thixotropy and stability in water that it is widely used as an excellent suspending agent and thickener in coatings, cosmetics, medicine and other industries.
[0004] Natural hectorite minerals are difficult to purify due to their small reserves and the large amount of impurities they usually contain. Artificially synthesized hectorite has fewer impurities, high purity, and can regulate interlayer charges, and the market demand is increasing. At present, the mature industrial hectorite synthesis method is mainly the hydrothermal method, which has many disadvantages. First, it needs to react under relatively high alkaline conditions, which will produce a lot of mixed wastewater containing waste alkali and salts that are difficult to handle; second, because hectorite has gel properties, it can form a viscous solid at a solid content of about 3%, and the solid content of the hydrothermal reaction is very low, usually difficult to exceed 7%, and the yield is low; third, due to the gel properties of hectorite, the aqueous solution is very viscous, and it is very difficult to filter and clean the product; fourth, the washed hectorite filter cake has a very low solid content, so it is very difficult to dry it and the cost is very high. It is precisely because of these shortcomings of the current hydrothermal method that the production process of hectorite is very complicated and cumbersome, with low output and high cost.
[0005] Based on the disadvantages of the current hydrothermal production of hectorite, this patent develops a new method for preparing hectorite by water vapor crystallization. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing laponite by water vapor crystallization, so as to solve the problems existing in the current hydrothermal method for preparing laponite, that is, the precursor gel for forming laponite is directly prepared by water vapor crystallization reaction to obtain laponite.
[0007] To achieve the above object, the present invention provides a method for preparing hectorite by water vapor crystallization, comprising the following steps:
[0008] S1. Weigh a certain amount of lithium salt, add a certain amount of deionized water to disperse and obtain a dispersion of lithium salt;
[0009] S2. Weigh a certain amount of magnesium salt into a beaker, add a certain amount of deionized water to dissolve to obtain a magnesium salt solution, and add a certain amount of alkali under stirring to react and obtain Mg(OH) 2 The precipitate was then filtered and washed with deionized water; the washed Mg(OH) 2 The wet filter cake is transferred to the lithium salt dispersion obtained in S1 and stirred to form a uniform mixed slurry;
[0010] S3, weigh a certain amount of water glass, add a certain amount of inorganic acid under stirring conditions, and react to obtain solid SiO 2 , then filtered and washed with deionized water; the washed SiO 2 The wet cake is transferred to the above S2 Mg(OH) 2 In a mixed slurry with lithium salt;
[0011] S4, rapidly stirring the mixed slurry of S3 within a certain temperature range to obtain a gel;
[0012] S5, crystallizing the gel obtained in S4 in water vapor at a certain temperature and pressure;
[0013] S6. Finally, the crystallized gel is dried to obtain hectorite.
[0014] Preferably, in the above-mentioned method for preparing hectorite by water vapor crystallization, the lithium salt in step S1 is lithium fluoride or lithium hydroxide; the magnesium salt in step S2 is magnesium chloride, magnesium sulfate or magnesium nitrate, and the alkali is sodium hydroxide, potassium hydroxide or ammonia water; the inorganic acid in step S3 is hydrochloric acid, sulfuric acid or nitric acid.
[0015] Preferably, in the above method for preparing laponite by water vapor crystallization, the gel prepared in step S4 has a molar ratio of Li:Mg:Si of (0.8-1.6):(5.2-5.6):8; and the solid content of the gel is 30-65%.
[0016] Preferably, in the above method for preparing hectorite by water vapor crystallization, the temperature range of step S4 is 30-90° C. and the time is 2-6 hours;
[0017] Preferably, in the above method for preparing laponite by water vapor crystallization, the water vapor crystallization in step S5 is carried out in a sealed environment with water vapor, with a water vapor pressure of 400-1900 kPa, a temperature of 150-210° C., and a time of 8-36 hours.
[0018] Preferably, in the above method for preparing hectorite by water vapor crystallization, the drying temperature of the gel after crystallization in step S6 is 105-150° C. and the drying time is 10-24 hours.
[0019] Preferably, in the above method for preparing hectorite by water vapor crystallization, the composition structure of the prepared hectorite is Li (0.4-0.8) [Li (0.4-0.8) Mg (5.2-5.6) Si 8 O 20 (OH·F) 4 ].
[0020] Therefore, the present invention adopts the above-mentioned method for preparing hectorite by water vapor crystallization to obtain the following technical effects:
[0021] (1) In the second and third steps of this method, Mg(OH) is generated 2 With SiO 2When the process is carried out, salt is also produced, but the composition of the produced salt is single. For example, in the second step, magnesium chloride is added to sodium hydroxide to mainly produce sodium chloride brine, and in the third step, water glass is added to sulfuric acid to mainly produce sodium sulfate brine. This single-composition brine is relatively easy to handle. This solves the problem that the wastewater produced by the hydrothermal method of producing lithium soapstone contains not only salt but also excessive alkali, and the treatment of this wastewater containing salt and alkali is very complicated.
[0022] (2) This method directly pre-reacts the reaction raw materials to form a gel. Since the gel has not yet turned into lithium soapstone, it can achieve a very high solid content. During the water vapor crystallization process, the gel can be loaded into a filter cloth with a certain pore size, placed on a tray with holes, and the tray is placed in a sealed oven to undergo a crystallization reaction through high-temperature and high-pressure water vapor. After the crystallization reaction is completed, the sealed oven is opened and the product in the tray is taken out, which solves the problem that the solid content of the hydrothermal production process is low, and if a gel product is formed in the reactor after the reaction is completed, it is difficult to discharge the material.
[0023] (3) This method directly uses raw materials for forming hectorite. After the water vapor crystallization reaction is completed, hectorite is directly obtained. For example, the molar ratio of Li:Mg:Si is 1:5.5:8 gel, the lithium salt is lithium fluoride, and the reaction formula is LiF+5.5Mg(OH) 2 +8SiO 2 →Li 0.5 [Li 0.5 Mg 5.5 Si 8 O 20 (OH) 3 F]+4H 2 O, after the reaction is completed, only the hectorite product and water are left, and no washing is required. The invention solves the problem that the hectorite product is prepared by hydrothermal reaction. Since the hectorite exists in water containing salt and alkali, the hectorite needs to be filtered and cleaned, and the hectorite aqueous solution is viscous, making it very difficult to filter and clean.
[0024] (4) The method obtains a hectorite gel product with a high solid content of 30-65%, which makes the drying cost very low. This solves the problem that the solid content of the filter cake obtained by filtering after washing the hydrothermal reaction hectorite is difficult to reach 20%, and the drying cost is very high.
[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A schematic diagram of a sealed stainless steel crystallization reactor filled with gel according to an embodiment of a method for preparing hectorite by water vapor crystallization of the present invention;
[0027] Figure 2The figure is a powder X-ray diffraction spectrum (XRD) of a sample prepared in an embodiment of a method for preparing laponite by water vapor crystallization according to the present invention. DETAILED DESCRIPTION
[0028] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings, and "multiple" generally includes at least two.
[0030] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such product or device. Without further restrictions, the elements defined by the sentence "comprises a ..." do not exclude the presence of other identical elements in the product or device including the elements.
[0031] Embodiment 1
[0032] The method for preparing hectorite by water vapor crystallization comprises the following steps:
[0033] ① Weigh 1.15 g (0.0274 mol) LiOH·H in a 500 mL beaker. 2 O, and then add 30g of deionized water and disperse evenly to obtain LiOH dispersion.
[0034] ② Weigh 18.24g (0.192mol) anhydrous MgCl 2 Put it in a 500mL beaker and add 100ml of deionized water to dissolve MgCl 2 Solution, add 288mL of 2mol·L -1 Ammonia water, fully react to obtain Mg(OH) 2 The precipitate was then filtered and washed with deionized water. 2 The wet filter cake was transferred to the above LiOH dispersion and stirred to form a uniform mixed slurry.
[0035] ③ Weigh 63.30 g of water glass (weight content: SiO 2 26%, Na 2 O8.2%)(containing SiO 2 0.274 mol), put it into a 500 mL beaker, add 55.81 mL of 3 mol·L -1 Hydrochloric acid, fully react to obtain SiO 2 The precipitation was then filtered and washed with deionized water. 2 The wet cake was transferred to the above Mg(OH) 2 Mixed slurry with LiOH.
[0036] ④ At a temperature of 55° C. and under reflux conditions, the mixed slurry was rapidly stirred and reacted for 3 hours to obtain a gel with a solid content of about 38%.
[0037] ⑤Put this gel into Figure 1 A sealed stainless steel crystallization reactor is shown, a certain amount of water is added to the bottom, the gel is placed in a sieve with a 200-mesh sieve, the crystallization reactor is heated to 200° C., and the crystallization reaction is carried out for 16 hours.
[0038] ⑥ After the crystallization reaction is completed, wait for the temperature of the crystallization reactor to drop to room temperature, open the reactor, take out the gel, and dry it at 110°C for 12 hours to obtain lithium soapstone with a composition of Li 0.4 [Li 0.4 Mg 5.6 Si 8 O 20 (OH) 4 ],
[0039] Figure 2 This is the X-ray diffraction pattern (XRD) of the hectorite powder prepared in Example 1. Strong diffraction peaks appear near 2-theta of 6.0°, 19.5°, 29.0°, 36.5°, 61.0° and 72.3°, and these diffraction peaks are completely the same as the characteristic diffraction peaks of hectorite, indicating that hectorite is prepared by this water vapor crystallization method.
[0040] Embodiment 2
[0041] The method for preparing hectorite by water vapor crystallization comprises the following steps:
[0042] ① Weigh 0.72 g (0.0274 mol) of LiF in a 500 mL beaker, add 30 g of deionized water, and disperse evenly to obtain a LiF dispersion.
[0043] ② Weigh 23.04 g (0.192 mol) of anhydrous MgSO 4 Put it in a 500mL beaker and add 100ml of deionized water to dissolve MgSO4 Solution, add 192mL of 2mol·L -1 NaOH solution, fully react to obtain Mg(OH) 2 The precipitate was then filtered and washed with deionized water. 2 The wet filter cake was transferred to the above LiF dispersion and stirred to form a uniform mixed slurry.
[0044] ③ Weigh 63.30 g of water glass (weight content: SiO 2 26%, Na 2 O8.2%)(containing SiO 2 0.274 mol), put it into a 500 mL beaker, add 55.81 mL of 3 mol·L -1 Hydrochloric acid, fully react to obtain SiO 2 The precipitation was then filtered and washed with deionized water. 2 The wet cake was transferred to the above Mg(OH) 2 In a mixed slurry with LiF.
[0045] ④ At a temperature of 60°C, under reflux conditions, the mixed slurry was rapidly stirred and reacted for 3 hours to obtain a gel with a solid content of about 38%. The molar ratio of Li:Mg:Si obtained was 1:5.5:8 gel, the lithium salt was lithium fluoride, and the reaction formula was as follows:
[0046] LiF+5.5Mg(OH) 2 +8SiO 2 →Li 0.5 [Li 0.5 Mg 5.5 Si 8 O 20 (OH) 3 F]+4H 2 O.
[0047] ⑤Put this gel into Figure 1 A sealed stainless steel crystallization reactor is shown, a certain amount of water is added to the bottom, the gel is placed in a sieve with a 200-mesh screen, the crystallization reactor is heated to 180° C., and the crystallization reaction is carried out for 24 hours.
[0048] ⑥ After the crystallization reaction is completed, wait for the temperature of the crystallization reactor to drop to room temperature, open the reactor, take out the gel, and dry it at 120°C for 12 hours to obtain lithium soapstone with a composition of Li 0.4 [Li 0.4 Mg 5.6 Si 8 O 20 (OH) 3.2 F 0.8 ], its XRD pattern is similar to Figure 2 Similarly, it is shown that hectorite was prepared by this water vapor crystallization method.
[0049] Comparative Example 1
[0050] Preparation of hectorite by hydrothermal method
[0051] First, you need to prepare LiOH and Mg(OH) 2 , diatomaceous earth and deionized water.
[0052] LiOH, Mg(OH) 2 Mix with deionized water in a ratio of 1:20:60, dissolve the magnesium source and lithium source in water first, and then mix them evenly by magnetic stirring. Add silicon source and diatomaceous earth to the mixture, and continue magnetic stirring to make the silicon source evenly dispersed in the solution.
[0053] The mixture was transferred into an autoclave, which was sealed and placed in an oven for heating at about 180° C. for 29 h.
[0054] After the reaction, the autoclave was naturally cooled to room temperature, and then the product was filtered and washed with deionized water for several times to remove residual salts and other impurities. The solid content of the filter cake after washing was 15%. The washed solid was dried at 120° C. for 24 hours, and X-ray diffraction (XRD) was used to observe that hectorite similar to that in Example 1 was obtained.
[0055] It can be seen that compared with the comparative example 1, the gel with a solid content of 38% is obtained in the examples 1 and 2 of the present application, and the subsequent drying time is 12 hours, which reduces the drying cost; while in the comparative example 1, the solid content of the filter cake after washing is 15%, and the washed solid is dried at 120°C for 24 hours to obtain the hectorite. The examples 1 and 2 of the present application reduce the drying cost by using the method of the present application; in the second and third steps, Mg(OH) is generated 2 With SiO 2 When the reaction is carried out, salt will be produced. However, the salt produced in the present embodiment has a single composition. For example, in the second step, magnesium chloride is added to sodium hydroxide to mainly produce sodium chloride brine, and in the third step, water glass is added to sulfuric acid to mainly produce sodium sulfate brine. This single composition brine is relatively easy to handle. In the second embodiment of the present application, the molar ratio of Li:Mg:Si obtained is 1:5.5:8 gel, and the lithium salt is lithium fluoride. The reaction formula is as follows: LiF+5.5Mg(OH) 2 +8SiO 2 →Li 0.5 [Li 0.5 Mg 5.5 Si 8 O 20 (OH) 3 F]+4H 2O, after the reaction is completed, only the hectorite product and water are generated, and no washing is required; while in Comparative Example 1, the hectorite product is prepared by hydrothermal reaction, and the hectorite needs to be filtered and cleaned. The present application does not require a washing step, which simplifies the preparation steps. The reaction raw materials are pre-reacted to form a gel. Since the gel has not yet become hectorite, a very high solid content can be achieved. The precursor gel of hectorite is directly obtained by water vapor crystallization to obtain hectorite. Hectorite can be obtained by simple preparation steps, which reduces many intermediate processing processes and improves the preparation efficiency compared to the hydrothermal method.
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing hectorite by water vapor crystallization, characterized in that: The steps include: S1. Weigh a certain amount of lithium salt, add a certain amount of deionized water to disperse and obtain a dispersion of lithium salt; S2, weigh a certain amount of magnesium salt and put it into a beaker, add a certain amount of deionized water to dissolve it to obtain a magnesium salt solution, add a certain amount of alkali under stirring conditions, react to obtain Mg(OH)2 precipitate, then filter it, and wash it with deionized water; transfer the washed Mg(OH)2 wet filter cake to the lithium salt dispersion obtained in S1, and stir to form a uniform mixed slurry; S3, weigh a certain amount of water glass, add a certain amount of inorganic acid under stirring conditions, react to obtain solid SiO2, then filter it and wash it with deionized water; the washed SiO2 wet filter cake is transferred to the mixed slurry of Mg(OH)2 and lithium salt in the above S2; S4, rapidly stirring the mixed slurry of S3 at a certain temperature range to obtain a gel; S5, crystallizing the gel obtained in S4 in water vapor at a certain temperature and pressure; S6. Finally, the crystallized gel is dried to obtain hectorite.
2. A method for preparing hectorite by water vapor crystallization according to claim 1, characterized in that: The lithium salt in step S1 is lithium fluoride or lithium hydroxide; the magnesium salt in step S2 is magnesium chloride, magnesium sulfate or magnesium nitrate; the alkali is sodium hydroxide, potassium hydroxide or ammonia water; the inorganic acid in step S3 is hydrochloric acid, sulfuric acid or nitric acid.
3. A method for preparing hectorite by water vapor crystallization according to claim 2, characterized in that: The gel prepared in step S4 has a molar ratio of Li:Mg:Si of (0.8-1.6):(5.2-5.6):8; and a solid content of the gel of 30-65%.
4. A method for preparing hectorite by water vapor crystallization according to claim 3, characterized in that: The temperature range of step S4 is 30-90° C. and the time is 2-6 hours.
5. A method for preparing hectorite by water vapor crystallization according to claim 4, characterized in that: The water vapor crystallization in step S5 is carried out in a sealed environment with water vapor, with a water vapor pressure of 400-1900 kPa, a temperature of 150-210° C., and a time of 8-36 hours.
6. A method for preparing hectorite by water vapor crystallization according to claim 5, characterized in that: In the step S6, the drying temperature of the crystallized gel is 105-150° C. and the drying time is 10-24 hours.
7. A method for preparing hectorite by water vapor crystallization according to claim 6, characterized in that: The composition structure of the prepared lithium laponite is Li (0.4-0.8) [Li (0.4-0.8) Mg (5.2-5.6) Si8O 20 (OH·F)4].
Citation Information
Patent Citations
Preparation method of high silica-alumina ratio Y type zeolite rich in secondary pores
CN103539151A
Method for preparing W molecular sieve by adopting steam assisted solid phase transformation
CN105523565A
Synthesis method for ZSM-11 molecular sieve with nano multi-stage pores
CN106430234A
Artificial hectorite and preparation method thereof
CN107857278A
Preparation method and application of molecular sieve catalyst
CN110882715A
Cited By
Magnetic hectorite and preparation method thereof
CN120420940A
A kind of magnetic hectorite and preparation method thereof
CN120420940B
Fe-N double-doped fluorine-free hectorite and synthesis method and application thereof, and wastewater treatment process
CN121819753A