Method for preparing ultrapure ammonia through adsorption rectification

Through the adsorption distillation method and the use of metal-organic framework material MIL-53, combined with temperature swing adsorption and low-temperature distillation, the problems of high energy consumption and low purity in the preparation of ultrapure ammonia in the existing technology have been solved, and high purity and high yield have been achieved. The preparation of ultrapure ammonia is suitable for industrial production.

CN118754150APending Publication Date: 2024-10-11KUNSHAN SHIPU NIANSHA AUXILIARY FACTORY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411176310.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing technology consumes huge amounts of energy and has low energy utilization when preparing ultrapure ammonia, making it difficult to achieve high purity and high yield simultaneously, resulting in product purity that remains stable below 99.9999% for a long time.

Method used

Adopting the adsorption distillation method, through the principles of adsorption concentration, adsorption desorption and shallow cold distillation separation, the metal organic framework material MIL-53 with a one-dimensional pore structure is used as the adsorbent, combining temperature swing adsorption and temperature changes to achieve the adsorption and removal of ammonia. Attached, impurities are further removed through low-temperature distillation to improve the purity of ammonia.

Benefits of technology

The preparation of high-purity ultrapure ammonia has been achieved. The product purity reaches 7N level. The yield is high, the energy consumption is low, the process is simple, and it is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of special gas production, in particular to a method for preparing ultra-pure ammonia through adsorption and rectification, which comprises the following steps: adsorption and concentration: removing solid particles from raw material ammonia, introducing the raw material ammonia with the temperature of-30-35 DEG C and the pressure of 0.5-1.5 MPa into an adsorption tower directly through a gas inlet pipeline, and introducing the raw material ammonia into the adsorption tower for adsorption and concentration; the ammonia serving as an adsorbate is adsorbed by an adsorbent filled in the adsorption tower, and non-adsorption phase components penetrating through a bed layer flow out; adsorption and desorption: the adsorbent for adsorbing ammonia obtained in the adsorption and concentration stage enters a separation kettle, the pressure is adjusted to 2.0-3.0 MPa, the temperature is adjusted to-20 DEG C to 80 DEG C, and the adsorbent is obtained from the bottom of the kettle; an adsorbed ammonia mixture escapes from the top of the kettle, and the adsorbent is subjected to adsorption concentration for recycling; an ammonia mixture flowing out in the adsorption and desorption process enters a shallow cooling rectifying still, oxygen, nitrogen, hydrogen and methane non-condensable gas impurities escape from the top of the rectifying still after rectifying operation, and ultra-pure ammonia with the purity of 7N level is obtained at the bottom of the rectifying still. According to the method, the problems of high energy consumption and low product purity in a traditional rectification method are solved, separation and purification are effectively realized, and an ultra-pure ammonia product with the purity stabilized at 99.9999% or above for a long time is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of special gas production, and in particular to a method for preparing ultrapure ammonia by adsorption distillation. Background Art

[0002] Ultrapure ammonia is a high-purity ammonia gas. It is a high-tech product that uses advanced equipment and technology to deeply process industrial liquid ammonia and make the ammonia purity reach 6N (99.9999%) or above. It is one of the main raw materials for solar photovoltaic and LED products and is usually used in the field of semiconductor manufacturing. The design and manufacture of ultrapure ammonia need to follow a series of strict standards and specifications to ensure quality and safety. Due to the late start of research on ultrapure ammonia in my country and the low technical level, domestic electronic grade ultrapure amino acids rely on imports.

[0003] At present, the production of ultra-pure ammonia mainly relies on flash evaporation, distillation and low-temperature distillation to remove trace amounts of water, oxygen, nitrogen and other impurities. However, the energy consumption is huge and the energy utilization rate is low. Although distillation is widely used in fields such as petrochemical refining, fine chemicals, and coal chemical industry, due to the phase change and the need for repeated heating and cooling in the form of heat exchange and mass transfer, its energy utilization rate is relatively low, and it is also impossible to improve the purity of the product while increasing the yield of the product. Therefore, whether it is azeotropic distillation or molecular distillation, it is impossible to effectively achieve separation and purification to obtain ultra-pure ammonia products with a long-term stable purity of more than 99.9999%. Summary of the invention

[0004] In order to effectively improve the above problems, the present application provides a method for preparing ultra-pure ammonia by adsorption distillation, which has the characteristics of high yield, high product purity, stable quality and low energy consumption.

[0005] The present application provides a method for preparing ultrapure ammonia by adsorption distillation, which adopts the following technical solution: A method for preparing ultrapure ammonia by adsorption distillation, comprising the following steps: adsorption concentration: after removing solid particles from raw ammonia, raw ammonia at a temperature of -30-35°C and a pressure of 0.5-1.5 MPa is directly introduced into an adsorption tower through an air inlet pipe, and ammonia as an adsorbate is adsorbed by an adsorbent filled in the adsorption tower, and non-adsorbed phase components pass through the bed layer and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 2.0-3.0MPa, the temperature is -20-80°C, and the adsorbent is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the adsorbent enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle.

[0006] By adopting the above technical scheme, the present application prepares ultra-pure ammonia by adsorption distillation based on the principles of adsorption concentration, adsorption desorption and shallow cold distillation separation. The raw ammonia is first decontaminated, and then ammonia adsorption is carried out through the adsorbent material. Most of the water and methane are removed by passing through the bed. Then, the adsorption and desorption steps are carried out by heating. Traditional temperature swing adsorption is adopted. It is necessary to realize the cyclic operation of adsorption and adsorption desorption regeneration through temperature changes. The adsorption and adsorption desorption are matched and balanced to obtain a dehydrated ammonia mixture. The purified ammonia after dehydration enters the low-temperature distillation again. Low-boiling point impurity components, such as oxygen, nitrogen, hydrogen, etc., overflow from the top of the distillation kettle, and an ultra-pure ammonia product with a purity of 7N is obtained at the bottom of the kettle.

[0007] In a specific embodiment, in the adsorption concentration step, the adsorption operation is performed at a temperature of -30-35°C and a pressure of 0.5-1.2 MPa.

[0008] By adopting the above technical solution, a certain range of temperature and pressure is set during the temperature-swing adsorption process, so that the adsorption capacity of the adsorbent is enhanced, the adsorption selectivity of ammonia is greater, and as much ammonia as possible is promoted to be adsorbed into the pores of the adsorbent.

[0009] In a specific embodiment, the adsorbent loaded in the adsorption tower for adsorption concentration is the metal organic framework material MIL-53.

[0010] By adopting the above technical solution, the adsorbent is a metal organic framework material MIL-53 with a one-dimensional pore structure. As a porous material with a flexible structure, the crystal framework is flexible and will "breathe" under the action of guest water molecules. Therefore, the material not only has a certain adsorption capacity for pure components such as ammonia, but also greatly enhances the adsorption selectivity of the material for ammonia and water mixtures.

[0011] In a specific embodiment, the preparation method of MIL-53 comprises the following steps: Mix chromium nitrate and terephthalic acid in proportion, add water to dissolve, stir for 1.5-3h, then add hydrofluoric acid dropwise and stir for 2-4h; After reacting at 120-180° C. for 72-120 hours, the reactor is cooled at a rate of 15-20° C. / min. After suction filtration, the obtained solid is dried and ground to obtain the metal organic framework material MIL-53.

[0012] By adopting the above technical scheme, chromium nitrate and terephthalic acid are stirred and mixed, hydrofluoric acid is added to adjust the coordination environment, and at a certain temperature, the raw materials are self-assembled and bridged in space to form a material with a one-dimensional pore structure with stable holes. The pore solvent is then removed through drying and activation to vacate the adsorption active sites in the pores, thereby greatly enhancing the adsorption selectivity of the material for ammonia for adsorption operations.

[0013] In a specific embodiment, the molar ratio of chromium nitrate, terephthalic acid, hydrogen fluoride and water is 1:1.5-2:1-3:300.

[0014] According to the coordination mode of the metal organic framework and the coordination structure formed, the molar ratio of the raw materials of the metal organic framework material is determined, which can promote the nucleation rate of the metal organic framework self-assembly and ensure the crystal quality. It is also beneficial to the synthesis yield of the metal organic framework and make the crystallization rate higher.

[0015] In a specific embodiment, the drying is vacuum drying at 80-100° C. for 2-4 hours.

[0016] Vacuum drying can prevent the metal organic framework pores from being blocked by solvents. Under certain temperature conditions, during the drying process, the solvent in the pores evaporates, opening up the metal organic framework active sites in the pores, further increasing the adsorption capacity and adsorption selectivity of ammonia.

[0017] In a specific embodiment, the non-adsorbed phase components obtained in the adsorption concentration step include water and methane, and the obtained methane is used as a refrigerant to provide cooling capacity for the shallow cold distillation step.

[0018] When methane is used as the refrigerant in the shallow cold distillation step, the present application can provide cooling capacity for the deoxygenation and removal of low-boiling impurity components steps, and the energy efficiency ratio is higher.

[0019] In a specific embodiment, the distillation operating conditions are a temperature of -30-48°C and an adsorption pressure of 3.5-4.0 MPa.

[0020] By adopting the above technical scheme, the purified ammonia gas after deep dehydration can be re-entered into the low-temperature distillation section through shallow cold distillation operation. Within a certain temperature and pressure range, low-boiling point impurity components, such as oxygen, nitrogen, hydrogen, etc., overflow from the top of the distillation kettle, and an ultra-pure ammonia product with a purity of 7N is obtained at the bottom of the kettle.

[0021] In summary, the present application includes at least one of the following beneficial technical effects: 1. The present application prepares ultra-pure ammonia by adsorption distillation based on the principles of adsorption concentration, adsorption desorption and shallow cold distillation separation. The raw ammonia is firstly decontaminated, and then ammonia is adsorbed by the adsorbent material, and most of the water and methane are removed by passing through the bed. Then, the adsorption and desorption steps are performed by heating. The traditional temperature swing adsorption is adopted, and the cyclic operation of adsorption and adsorption desorption regeneration needs to be realized by temperature change. The adsorption and adsorption desorption are matched and balanced to obtain a dehydrated ammonia mixture. The purified ammonia after dehydration enters the low-temperature distillation again, and the low-boiling point impurity components, such as oxygen, nitrogen, hydrogen, etc., overflow from the top of the distillation kettle, and an ultra-pure ammonia product with a purity of 7N is obtained at the bottom of the kettle.

[0022] 2. The adsorbent selected is the metal organic framework material MIL-53 with a one-dimensional pore structure. As a porous material with a flexible structure, the crystal framework is flexible and will "breathe" under the action of guest water molecules. Therefore, the material not only has a certain adsorption capacity for pure components such as ammonia, but also greatly enhances the adsorption selectivity of the material for ammonia and water mixtures.

[0023] 3. Through the shallow cold distillation operation, the purified ammonia after deep dehydration can enter the low-temperature distillation section again. Within a certain temperature and pressure range, low-boiling point impurity components, such as oxygen, nitrogen, hydrogen, etc., overflow from the top of the distillation kettle, and an ultra-pure ammonia product with a purity of 7N is obtained at the bottom of the kettle. DETAILED DESCRIPTION

[0024] In the present application, chromium nitrate is chromium nitrate nonahydrate, purchased from Guangzhou Sanchang Chemical Co., Ltd., terephthalic acid was purchased from Jinan Huijinchuan Trading Co., Ltd.; hydrofluoric acid is 40% reagent grade hydrofluoric acid purchased from Foshan Nanhai Shuangfluorine Chemical Co., Ltd.; other raw materials can be obtained commercially.

[0025] Preparation Example Preparation Example 1 The preparation method of the metal organic framework material MIL-53 (Cr) is as follows: add chromium nitrate, terephthalic acid and water into a reaction kettle, stir ultrasonically for 1.5 hours, add hydrofluoric acid dropwise, and stir for another 2 hours; wherein the molar ratio of chromium nitrate, terephthalic acid, hydrogen fluoride and water is 1:1.5:1:300, and then react at 120°C for 72 hours; after the reaction is completed, cool the reaction kettle at a rate of 15°C / min, filter with an air pump, put the solid into a vacuum oven at 80°C and dry it for 2 hours, and then grind the dried solid to obtain the metal organic framework material MIL-53 (Cr).

[0026] Preparation Example 2 The preparation method of the metal organic framework material MIL-53 (Cr) is as follows: add chromium nitrate, terephthalic acid and water into a reaction kettle, stir ultrasonically for 2.5 hours, add hydrofluoric acid dropwise, and stir for another 3 hours; wherein the molar ratio of chromium nitrate, terephthalic acid, hydrogen fluoride and water is 1:1.5-2:1-3:300, and then react at 160°C for 96 hours; after the reaction is completed, cool the reaction kettle at a rate of 20°C / min, filter with an air pump, put the solid into a vacuum oven at 100°C and dry for 3 hours, and then grind the dried solid to obtain the metal organic framework material MIL-53 (Cr).

[0027] Preparation Example 3 The preparation method of the metal organic framework material MIL-53 (Cr) is as follows: add chromium nitrate, terephthalic acid and water into a reaction kettle, stir ultrasonically for 3 hours, add hydrofluoric acid dropwise, and stir for another 4 hours; wherein the molar ratio of chromium nitrate, terephthalic acid, hydrogen fluoride and water is 1:1.5-2:1-3:300, and then react at 180°C for 120 hours; after the reaction is completed, cool the reaction kettle at a rate of 20°C / min, filter with an air pump, put the solid into a vacuum oven at 100°C and dry for 4 hours, and then grind the dried solid to obtain the metal organic framework material MIL-53 (Cr).

[0028] Preparation Example 4 The preparation method of the metal organic framework material MIL-53 (Cr) is as follows: add chromium nitrate, terephthalic acid and water into a reaction kettle, stir ultrasonically for 3 hours, add hydrofluoric acid dropwise, and stir for another 4 hours; wherein the molar ratio of chromium nitrate, terephthalic acid, hydrogen fluoride and water is 1:2:3:300, and then react at 180°C for 120 hours; after the reaction is completed, cool the reactor at a rate of 20°C / min, filter with an air pump, put the solid into a vacuum oven at 100°C and dry for 4 hours, and then grind the dried solid to obtain the metal organic framework material MIL-53 (Cr).

[0029] Preparation Example 5 The preparation method of the metal organic framework material MIL-53 (Cr) is as follows: add chromium nitrate, terephthalic acid and water into a reaction kettle, stir ultrasonically for 3 hours, add hydrofluoric acid dropwise, and stir for another 4 hours, wherein the molar ratio of chromium nitrate, terephthalic acid, hydrogen fluoride and water is 2:1.5:3:300, and then react at 180°C for 120 hours; after the reaction is completed, cool the reactor at a rate of 20°C / min, filter with an air pump, put the solid into a vacuum oven at 100°C and dry for 4 hours, and then grind the dried solid to obtain the metal organic framework material MIL-53 (Cr).

[0030] Example 1 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, and then directly introduce raw ammonia at a temperature of -30°C and a pressure of 0.5MPa into the adsorption tower through the air inlet pipe. In the adsorption tower, adsorption is carried out under the conditions of a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 1 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 2.0 MPa, the temperature is -20°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle, with a yield of more than 99%.

[0031] Example 2 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass the raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, then pass the raw ammonia at a temperature of 35°C and a pressure of 1.5MPa directly into the adsorption tower through the air inlet pipe, and adsorption is carried out in the adsorption tower at a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 1 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 3.0 MPa, the temperature is 80°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle, with a yield of more than 99%.

[0032] Example 3 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, then introduce raw ammonia at a temperature of 35°C and a pressure of 1.5MPa directly into the adsorption tower through the air inlet pipe, and adsorption is carried out in the adsorption tower at a temperature of 55°C and a pressure of 1.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 1 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 3.0 MPa, the temperature is 80°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle, with a yield of more than 99%.

[0033] Example 4 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass the raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, and then directly introduce the raw ammonia at a temperature of 35°C and a pressure of 1.5MPa into the adsorption tower through the air inlet pipe. In the adsorption tower, adsorption is carried out under the conditions of a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 2 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 3.0 MPa, the temperature is 80°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle, with a yield of more than 99%.

[0034] Example 5 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass the raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, and then directly introduce the raw ammonia at a temperature of 35°C and a pressure of 1.5MPa into the adsorption tower through the air inlet pipe. In the adsorption tower, adsorption is carried out under the conditions of a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 3 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 3.0 MPa, the temperature is 80°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle, with a yield of more than 99%.

[0035] Example 6 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, then introduce raw ammonia at a temperature of 35°C and a pressure of 1.5MPa directly into the adsorption tower through the air inlet pipe, and adsorption is carried out in the adsorption tower at a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 4 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 3.0 MPa, the temperature is 80°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle, with a yield of more than 99%.

[0036] In Examples 1-6 of the present application, a method for preparing ultra-pure ammonia by adsorption distillation has mild reaction conditions, large adsorption capacity of the adsorbent, high efficiency, low energy consumption in the adsorption distillation process, high product purity, and expanded the difference in adsorbent selectivity between water and ammonia components. The operation is relatively flexible; separation and purification are effectively achieved to obtain an ultra-pure ammonia product with a long-term stable purity of 7N level, the process is simple, and can be used for industrial production.

[0037] Example 7 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, then introduce raw ammonia at a temperature of 35°C and a pressure of 1.5MPa directly into the adsorption tower through the air inlet pipe, and adsorption is carried out in the adsorption tower at a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 5 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 3.0 MPa, the temperature is 80°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle, with a yield of more than 99%.

[0038] The present embodiment provides a method for preparing ultrapure ammonia by adsorption distillation. The reaction conditions are mild, the adsorption capacity of the adsorbent is smaller than that of Examples 1-6, and the adsorption and desorption time is longer. The applicant believes that the purity of MIL-53 prepared in Preparation Example 5 is not high, there are more impurities, and the adsorption effective components are less. However, the adsorption distillation process has low energy consumption, high product purity, and expands the difference in adsorbent selectivity between water and ammonia components. The operation is relatively flexible; separation and purification are effectively achieved to obtain an ultrapure ammonia product with a long-term stable purity of 7N level. The process is simple and can be used for industrial production.

[0039] Comparative Example 1 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass the raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, then pass the raw ammonia at a temperature of 50°C and a pressure of 1.5MPa directly into the adsorption tower through the air inlet pipe, and adsorption is carried out in the adsorption tower at a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 1 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 3.0 MPa, the temperature is 80°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia is obtained at the bottom of the distillation kettle with a yield of more than 99%.

[0040] Compared with Example 1, as the adsorption temperature increases, the adsorption amount of the adsorbent decreases, and the yield of ultra-pure ammonia decreases. The applicant believes that this may be because the metal organic framework adsorption is an exothermic reaction, and the higher the ambient temperature, the lower the adsorption amount. Therefore, it is not appropriate to exceed the temperature range of this application.

[0041] Comparative Example 2 A method for preparing ultrapure ammonia by adsorption distillation comprises the following steps: Adsorption concentration: use a metering pump to pass the raw industrial ammonia from the raw material storage tank through a filter to remove solid particles, then pass the raw ammonia at a temperature of 35°C and a pressure of 1.5MPa directly into the adsorption tower through the air inlet pipe, and adsorption is carried out in the adsorption tower at a temperature of -30°C and a pressure of 0.5MPa. The ammonia adsorbate is adsorbed by the MIL-53 prepared in Preparation Example 1 loaded in the adsorption tower, while the non-adsorbed phase components water and methane pass through the bed and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 0.5MPa, the temperature is -35°C, and the MIL-53 desorbed with ammonia is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the MIL-53 enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia is obtained at the bottom of the distillation kettle with a yield of more than 99%.

[0042] Comparative Example 3 Liquid phase adsorption: Use a metering pump to remove solid particles from the raw material storage tank through a filter, and then introduce the raw material ammonia at a temperature of 35°C and a pressure of 1.5MPa directly into the adsorption tower through the air inlet pipe. In the adsorption tower, adsorption is carried out under the conditions of a temperature of -30°C and a pressure of 0.5MPa. Water is adsorbed as an adsorbate by the 13X series molecular sieve loaded in the adsorption tower as an adsorbent. Water and trace impurity components are adsorbed as adsorbates, and liquid ammonia as a non-adsorbed phase passes through the bed and flows out from the bottom of the adsorption tower; Shallow cold distillation: The ammonia mixture flowing out during the liquid phase adsorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and pure ammonia is obtained at the bottom of the distillation kettle with a yield of less than 99%.

[0043] Compared with Example 2, Comparative Example 3 cannot effectively achieve separation and purification to obtain an ultra-pure ammonia product with a long-term stable purity of 7N level. The applicant believes that this may be because the molecular sieve is used as an adsorption material to adsorb moisture. Since some dissolved liquid ammonia is also entrained in the raw ammonia, hydrogen bonds between ammonia and water interact with each other. Therefore, the pore size of the molecular sieve is uneven and there are no active sites in the pores. The effect of the molecular sieve in removing water is weak, and the purity of the product is reduced.

[0044] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing ultrapure ammonia by adsorption distillation, characterized in that , including the following steps: adsorption concentration: after removing solid particles from the raw ammonia, the raw ammonia at a temperature of -30-35°C and a pressure of 0.5-1.5MPa is directly introduced into the adsorption tower through the air inlet pipe. In the adsorption tower, ammonia as an adsorbate is adsorbed by the adsorbent filled in the adsorption tower, and the non-adsorbed phase components pass through the bed layer and flow out; Adsorption and desorption: The adsorbent adsorbed with ammonia obtained in the adsorption and concentration stage enters the separation kettle, the pressure is adjusted to 2.0-3.0MPa, the temperature is -20-80°C, and the adsorbent is obtained from the bottom of the kettle; the adsorbed ammonia mixture escapes from the top of the kettle, and the adsorbent enters the adsorption and concentration again for recycling; Shallow cold distillation: The ammonia mixture flowing out during the adsorption and desorption process enters a shallow cold distillation kettle. After the distillation operation, oxygen, nitrogen, hydrogen, and methane non-condensable gas impurities escape from the top of the distillation kettle, and ultra-pure ammonia with a purity of 7N grade is obtained at the bottom of the distillation kettle.

2. The method for preparing ultrapure ammonia by adsorption distillation according to claim 1, characterized in that: In the adsorption concentration step, the adsorption operation is performed at a temperature of -30-35°C and a pressure of 0.5-1.2 MPa.

3. The method for preparing ultrapure ammonia by adsorption distillation according to claim 1, characterized in that: The adsorbent filled in the adsorption tower for adsorption concentration is the metal organic framework material MIL-53.

4. The method for preparing ultrapure ammonia by adsorption distillation according to claim 3, characterized in that: The preparation method of MIL-53 comprises the following steps: Mix chromium nitrate and terephthalic acid in proportion, add water to dissolve, stir for 1.5-3h, then add hydrofluoric acid dropwise and stir for 2-4h; After reacting at 120-180° C. for 72-120 hours, the reactor is cooled at a rate of 15-20° C. / min. After suction filtration, the obtained solid is dried and ground to obtain the metal organic framework material MIL-53.

5. The method for preparing ultrapure ammonia by adsorption distillation according to claim 4, characterized in that: The molar ratio of the chromium nitrate, terephthalic acid, hydrogen fluoride and water is 1:1.5-2:1-3:

300.

6. The method for preparing ultrapure ammonia by adsorption distillation according to claim 4, characterized in that: The drying is vacuum drying at 80-100° C. for 2-4 hours.

7. The method for preparing ultrapure ammonia by adsorption distillation according to claim 1, characterized in that: The non-adsorbed phase components obtained in the adsorption concentration step include water and methane, and the obtained methane is used as a refrigerant to provide cold capacity for the shallow cold distillation step.

8. The method for preparing ultrapure ammonia by adsorption distillation according to claim 1, characterized in that: The distillation operating conditions are: temperature -30-48°C and adsorption pressure 3.5-4.0MPa.

Citation Information

Patent Citations

  • Full-temperature-range adsorption, extraction, deep dehydration and impurity-removing purification method for ultrapure ammonia

    CN107777703A

  • Method for recycling ammonia from ammonia-containing gas or ammonia-containing liquid, ammonia recycling device and ammonia gas storage device

    CN117580804A