Method for removing potassium from lithium-containing leachate
Through the method of freezing sodium precipitation and potassium precipitation, combined with the potassium thenardite conversion method, the potassium content in the lithium-containing leachate can be effectively reduced, solving the problem of uneconomical and efficient potassium removal in the existing technology, and achieving high potassium removal rate and elemental content. Protection of the quality of flour.
Patent Information
- Application Number
- CN202410979495.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
AI Technical Summary
The existing methods for removing potassium from lithium-containing leach solutions are not economical and efficient, and have a great impact on the quality of Yuanming powder, making it difficult to achieve industrial production.
By freezing the lithium-containing leaching solution for sodium precipitation, sodium sulfate decahydrate and the cold eluate are obtained. Potassium sulfate is then added to the cold eluate to precipitate potassium. Potassium sulfate is prepared using the potassium mirabilite conversion method. The potassium precipitation is repeated until a high temperature is reached. Potassium removal rate.
It has achieved an efficient and economical reduction of the potassium content in the lithium-containing leach solution, with a potassium removal rate of over 80%, and made full use of potassium mirabilite to protect the quality of Yuanming powder.
Smart Images

Figure BDA0004955958280000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium hydroxide production, and in particular to a method for removing potassium from a lithium-containing leaching solution. Background Art
[0002] The lithium-containing leachate is a solution obtained by calcining lithium clay by sulfate method, leaching with water, and filtering and separating. It is a coexistence system of lithium sulfate, potassium sulfate, and sodium sulfate solution. + The concentration is 10-15 g / L, Na + The concentration is 10~30g / L, K + The concentration is 20-50g / L. The solubility of sodium in the system varies at different temperatures. It can be separated by cooling and recrystallized to obtain sodium sulphate, while lithium and potassium are difficult to separate, which is related to the process selection and manufacturing cost of lithium products.
[0003] At present, there are precipitation, extraction, resin, electrodialysis and other methods for removing potassium from solutions. For example, patent CN113387374A uses iron salt and potassium to generate jarosite, and patent CN112575339A uses electrodialysis to remove sodium and potassium, but these methods are not economical and efficient and cannot be industrialized. Patent CN112978769A uses the byproduct sodium sulfate to take away part of the potassium in the solution, thereby reducing the potassium content in the production system, but it affects the quality of sodium sulfate and affects sales. Summary of the invention
[0004] The object of the present invention is to provide a method for removing potassium from a lithium-containing leaching solution, which is economical, efficient and can be industrialized.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for removing potassium from a lithium-containing leaching solution, comprising the following steps:
[0007] A method for removing potassium from a lithium-containing leachate, comprising the following steps:
[0008] Freezing the lithium-containing leaching solution for sodium precipitation to obtain sodium sulfate decahydrate and cold precipitation liquid;
[0009] adding potassium sulfate to the cold separation liquid to precipitate potassium, thereby obtaining glauber's salt and potassium removal liquid;
[0010] When potassium is precipitated, K + with Na + The concentration ratio is 3:1.
[0011] Preferably, the lithium-containing leachate is a leachate obtained by extracting lithium from spodumene or clay ore by sulfate roasting.
[0012] Preferably, the lithium-containing leaching solution contains Li + With K + The concentration ratio is 1:2~1:6.
[0013] Preferably, the frozen sodium precipitation is to freeze the lithium-containing leaching solution to -7 to -10°C, wherein the Na + The concentration is 5~35g / L.
[0014] Preferably, the number of potassium precipitations is ≥1. When the number of potassium precipitations is ≥2, the potassium precipitation step comprises: adding potassium sulfate to the cold separation liquid for the first potassium precipitation, and obtaining a first glauber'ite and a first potassium removal liquid after separation; adding potassium sulfate to the first potassium removal liquid for the second potassium precipitation, and separating to obtain a second glauber'ite and a second potassium removal liquid; and repeating the potassium precipitation until the potassium removal liquid is obtained.
[0015] Preferably, each time potassium is precipitated, the K in the resulting mixed solution after adding potassium sulfate is + with Na + The concentration ratio is 3:1.
[0016] Preferably, the temperature of each potassium precipitation is independently -7 to -10°C.
[0017] Preferably, after the potassium precipitation is completed, the potassium glauberite obtained from the stepwise potassium precipitation is mixed, and potassium sulfate solid is prepared by the sodium glauberite conversion method, which is reused in the potassium precipitation step.
[0018] The invention provides a method for removing potassium from a lithium-containing leachate, wherein the lithium-containing leachate is subjected to freezing and sodium precipitation to obtain sodium sulfate decahydrate and a cold precipitation liquid, potassium sulfate solid is added to the cold precipitation liquid to make the K and Na ion concentration ratio in the solution reach 3:1, and 3K2SO4·Na2SO4 glauberite crystals (which only dissolve but do not decompose in the solution) are obtained by reaction, and the present invention adds potassium salt to the lithium-containing leachate to make the K and Na ion concentrations reach 3:1, and precipitates K in the leachate in the form of glauberite through potassium sulfate precipitation to obtain a lithium sulfate solution with a low potassium impurity content, thereby achieving a high potassium removal rate of the lithium-containing leachate. The present invention can use the potassium sulfate produced by the glauberite obtained by removing potassium from the leachate to form a composite salt with sodium sulfate in the lithium-containing leachate to precipitate glauberite, thereby reducing the potassium content in the leachate, and the glauberite can be used to prepare potassium sulfate through a glauberite conversion method, so that K in the lithium-containing leachate is fully utilized, and the potassium removal rate of the leachate is greater than 80%. DETAILED DESCRIPTION
[0019] The present invention provides a method for removing potassium from a lithium-containing leaching solution, comprising the following steps:
[0020] Freezing the lithium-containing leaching solution for sodium precipitation to obtain sodium sulfate decahydrate and cold precipitation liquid;
[0021] adding potassium sulfate to the cold separation liquid to precipitate potassium, thereby obtaining glauber's salt and potassium removal liquid;
[0022] When potassium is precipitated, K + with Na + The concentration ratio is 3:1.
[0023] In the present invention, the lithium-containing leachate is preferably a leachate obtained by extracting lithium from spodumene or clay ore by sulfate roasting. The present invention has no particular limitation on the source of the lithium-containing leachate, which can be obtained in a manner known in the art.
[0024] In the present invention, the lithium-containing leaching solution contains Li + With K + The concentration ratio is preferably 1:2 to 1:6, more preferably 1:2.4 to 3.0.
[0025] In the present invention, the frozen sodium precipitation is preferably carried out by freezing the lithium-containing leachate to -7 to -10°C, more preferably -7 to -8°C, at room temperature. + The concentration is preferably 5 to 35 g / L, more preferably 10 to 20 g / L.
[0026] The present invention reduces the sodium ion concentration in the solution through the freezing sodium precipitation process, so as to reduce the amount of potassium sulfate used.
[0027] After completing the freezing sodium precipitation, the present invention preferably separates the obtained product into solid and liquid to obtain sodium sulfate decahydrate and cold precipitation liquid; the present invention has no special limitation on the solid-liquid separation, and it can be carried out according to the process well known in the art; in the embodiment of the present invention, it is specifically filtration.
[0028] In the present invention, the number of potassium precipitations is ≥ 1. When the number of potassium precipitations is ≥ 2, the potassium precipitation step includes: adding potassium sulfate to the cold separation liquid for the first potassium precipitation, and obtaining a first glauber's salt and a first potassium removal liquid after separation; adding potassium sulfate to the first potassium removal liquid for the second potassium precipitation, and separating to obtain a second glauber's salt and a second potassium removal liquid; repeating the potassium precipitation until a potassium removal liquid is obtained. The present invention has no special limitation on the separation, and any solid-liquid separation method well known in the art can be used; in an embodiment of the present invention, it is specifically filtration. The present invention preferably determines the number of potassium precipitations based on the potassium removal rate, so that the potassium removal rate is greater than 80%.
[0029] The method of repeatedly precipitating potassium in the present invention is to add potassium sulfate to the second potassium removal liquid for the third potassium precipitation, separate to obtain a third glauber's salt and a third potassium removal liquid, add potassium sulfate to the third potassium removal liquid for the fourth potassium precipitation, separate to obtain a fourth glauber's salt and a fifth potassium removal liquid, and repeat the potassium precipitation in this way; the potassium removal liquid finally obtained is a lithium sulfate solution.
[0030] In the present invention, each time potassium is precipitated, potassium sulfate is added to the resulting mixed solution. + with Na + The concentration ratio is preferably 3: 1. The present invention limits the amount of potassium sulfate used in each potassium precipitation according to the sodium ion concentration.
[0031] In the present invention, the temperature of each potassium precipitation is preferably -7 to -10°C, more preferably -7 to -8°C; the present invention preferably freezes the mixed solution after adding potassium sulfate from room temperature to the potassium precipitation temperature to complete potassium precipitation.
[0032] In the present invention, after the potassium precipitation is completed, the potassium glauberite obtained by the stepwise potassium precipitation is mixed, and potassium sulfate solid is prepared by the sodium glauberite conversion method, and is reused in the potassium precipitation step.
[0033] The present invention has no particular limitation on the specific steps and conditions for preparing potassium sulfate by the mirabilite conversion method, and the potassium sulfate can be prepared according to methods well known in the art.
[0034] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0035] The lithium-containing leaching solution used in the following examples is the leaching solution after lithium is extracted from clay ore by sulfate roasting, wherein Li + 、Na + and K + The concentrations are shown in Table 1.
[0036] Example 1
[0037] 1L of lithium-containing leaching solution after lithium extraction from clay ore was taken, frozen to -7°C from room temperature, filtered, and 430g of sodium sulfate decahydrate and 675mL of cold precipitation liquid were obtained, and 1L of cold precipitation liquid was obtained according to the steps;
[0038] Take 1L of the cold precipitate obtained above, add 142g of potassium sulfate solid, so that the K + with Na + The concentration ratio was 3:1, and the resulting mixture was frozen from room temperature to -7°C to precipitate potassium, and filtered to obtain 138 g of potassium glauberite and 960 mL of potassium removal solution (Na + Concentration is 5g / L);
[0039] To the prepared glauber's salt, 0.67 times the total mass of potassium chloride and 1.46 times the total mass of water were added, the mixture was stirred at 60° C. for 30 min, and filtered to separate to obtain potassium sulfate solid.
[0040] Example 2
[0041] 1L of lithium-containing leaching solution after lithium extraction from clay ore was taken, frozen to -7°C from room temperature, filtered, and 442g of sodium sulfate decahydrate and 668mL of cold precipitation liquid were obtained, and 1L of cold precipitation liquid was obtained according to the steps;
[0042] Take 1L of the cold precipitate obtained above, add 53g of potassium sulfate solid obtained according to Example 1, so that K in the mixed solution + with Na + The concentration ratio was 3:1, and the resulting mixed solution was frozen from room temperature to -7°C for the first potassium precipitation, filtered, and 50 g of the first potassium sulfate and 972 mL of the first potassium removal solution (Na + Concentration is 10g / L);
[0043] The first potassium removal solution was mixed with 110.3 g potassium sulfate so that K + with Na + The concentration ratio is 3:1, and the obtained mixed solution is frozen from room temperature to -8°C for second potassium precipitation, and filtered to obtain 11.2g of second potassium sulfate and 920mL of second potassium removal solution;
[0044] The first glauber's salt and the second glauber's salt were mixed, and then potassium sulfate solid was prepared by the glauber's salt conversion method according to Example 1.
[0045] Example 3
[0046] 1L of lithium-containing leaching solution after lithium extraction from clay ore was taken, frozen to -7°C from room temperature, filtered, and 440g of sodium sulfate decahydrate and 670mL of cold precipitation liquid were obtained, and 1L of cold precipitation liquid was obtained according to the steps;
[0047] Take 1L of the cold precipitate obtained above, add 155g of potassium sulfate solid obtained according to the method of Example 2, so that K in the mixed solution + with Na + The concentration ratio was 3:1, and the resulting mixed solution was frozen from room temperature to -7°C for the first potassium precipitation, filtered, and 147 g of the first potassium sulfate and 975 mL of the first potassium removal solution (Na + Concentration is 15g / L);
[0048] The first potassium removal solution was mixed with 166 g potassium sulfate so that K + with Na + The concentration ratio is 3:1, and the obtained mixed solution is frozen from room temperature to -10°C for second potassium precipitation, and filtered to obtain 8.6g of second glauberite and 920mL of second potassium removal solution;
[0049] The first glauber's salt and the second glauber's salt were mixed, and then potassium sulfate solid was prepared by the glauber's salt conversion method according to Example 1.
[0050] Table 1 Potassium removal effect of Examples 1 to 3
[0051]
[0052] As shown in Table 1, the method of adding potassium sulfate and sodium sulfate to the lithium-containing leaching solution system to precipitate potassium sulfate reduces the potassium content in the leaching solution, and the potassium removal rate is greater than 80%.
[0053] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for removing potassium from a lithium-containing leachate, characterized in that: The following steps are involved: Freezing the lithium-containing leachate to separate out sodium to obtain sodium sulfate decahydrate and a cold precipitation liquid; adding potassium sulfate to the cold precipitated liquid to precipitate potassium, thereby obtaining glauberite and a potassium-removing liquid; When potassium is precipitated, K + with Na + The concentration ratio is 3:
1.
2. The method according to claim 1, characterized in that The lithium-containing leachate is the leachate obtained by extracting lithium from spodumene or clay ore through a sulfate roasting method.
3. The method according to claim 1 or 2, characterized in that Li in the lithium-containing leachate + With K + The concentration ratio is 1:2 to 1:
6.
4. The method according to claim 1, wherein The freezing sodium precipitation is to freeze the lithium-containing leachate to -7 to -10 ° C. + The concentration is 5-35g / L.
5. The method according to claim 1, wherein The number of potassium precipitations is ≥1. When the number of potassium precipitations is ≥2, the potassium precipitation step comprises: adding potassium sulfate to the cold separation liquid for a first potassium precipitation, and obtaining a first glauberite and a first potassium removal liquid after separation; adding potassium sulfate to the first potassium removal liquid for a second potassium precipitation, and separating to obtain a second glauberite and a second potassium removal liquid; and repeating the potassium precipitation until the potassium removal liquid is obtained.
6. The method according to claim 1 or 5, characterized in that Each time potassium is precipitated, the K in the resulting mixed solution after adding potassium sulfate is + with Na + The concentration ratio is 3:
1.
7. The method according to claim 1 or 5, characterized in that The temperature of each potassium precipitation is independently -7 to -10°C.
8. The method according to claim 1 or 5, characterized in that After the potassium precipitation is completed, the potassium sulfate obtained from the separate potassium precipitation steps is mixed, and potassium sulfate solid is prepared by the sodium sulfate conversion method, which is then reused in the potassium precipitation step.