Tempered glass ceramic, cover plate glass, electronic equipment and glass device
By using zinc-aluminum spinel-magnesia-aluminum spinel solid solution to strengthen glass ceramics on the cover glass of electronic equipment, a specific stress distribution structure is formed, which solves the problem that the cover glass of electronic equipment is susceptible to scratches and achieves a better Long service life and better user experience.
Patent Information
- Application Number
- CN202410740145.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
AI Technical Summary
The cover glass of existing electronic equipment is easily scratched by dust, dust and sharp objects during use, resulting in scratches and a decrease in optical performance, affecting the display effect, and the existing anti-scratch coating is easily scratched under friction and tremor. Wear failure.
Strengthened glass ceramics that use zinc-aluminum spinel-magnesia-aluminum spinel solid solution as the main crystal phase form a compressive stress layer and internal tensile stress on the surface to meet a specific stress distribution structure and improve the scratch resistance of the glass.
Even if the anti-scratch coating wears away, the reinforced glass ceramic still maintains excellent anti-scratch effect, significantly reducing the probability and impact of scratches, extending the service life of electronic devices and improving user experience.
Smart Images

Figure CN118754429A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of microcrystalline glass, and in particular to a strengthened glass ceramic, a cover glass, an electronic device and a glass device. Background Art
[0002] With the rapid development of the electronic information industry, electronic devices such as smart wearables, smart phones, and computer tablets are becoming more and more popular. In the iteration of electronic devices, many new materials are used in the design and manufacture of electronic devices. Glass-ceramic materials are gradually used in electronic devices due to their excellent mechanical properties (such as flexural strength, fracture toughness, surface hardness, etc.) and good light transmittance, such as display screen cover glass, camera protection cover glass, or back cover glass of electronic devices.
[0003] In daily use, the cover glass on the surface of electronic devices, in addition to facing destructive damage caused by falling, impact, extrusion, etc., will also face problems such as scratches caused by dust and dirt (such as sand and gravel). For example, after long-term use, the display screen cover glass of electronic devices is easily contaminated with dust or dirt (such as sand and gravel). Its main component is silicon dioxide, and its Mohs hardness level is about 6 to 7. Most of the existing cover glasses have a lower hardness than silicon dioxide materials. When fingers are swiped on the screen cover glass contaminated with dust or dirt, it will drive the dust or dirt to rub on the cover glass. In the long run, the surface of the cover glass will be scratched, leaving scratches, and producing a particularly rough feel. In addition, when the scratches are serious, it will directly affect the display effect of the screen, because when the scratches are serious, the optical properties of the screen cover glass will be greatly affected, such as significantly increasing its haze, thereby affecting the display effect of the screen. In some other cases, during use, the cover glass is directly scratched by a sharp object, leaving scratches. Summary of the invention
[0004] At present, the main method to enhance the scratch resistance of cover glass is to spin-coat a protective film coating on the glass surface, prepare an organic film, etc., to improve the scratch resistance of the glass. In order not to affect the display effect and normal touch use of the electronic display screen, the scratch-resistant coating is usually set very thin. Long-term friction, vibration cracking, etc. can easily cause the coating to be worn away, which in turn makes it unable to play a role in improving the scratch resistance of the cover glass.
[0005] In view of this, the purpose of this application is to provide a reinforced glass ceramic material with excellent scratch resistance. The reinforced glass ceramic is used as the display screen cover glass of electronic equipment. Even if the scratch-resistant coating on its surface is worn away, it can still maintain excellent scratch resistance. The reinforced glass ceramic provided in this application can significantly reduce the probability of the display screen cover glass being scratched by hard objects, reduce the adverse effects of scratches caused by scratches, and help to improve the service life of electronic equipment and user experience.
[0006] In order to achieve the above objectives, this application provides the following technical solutions:
[0007] In a first aspect, a reinforced glass ceramic is provided, wherein the reinforced glass ceramic comprises a main crystalline phase of zinc aluminum spinel-magnesium aluminum spinel solid solution and a secondary crystalline phase of zirconium oxide;
[0008] The reinforced glass-ceramic has a compressive stress layer on the surface and tensile stress inside; the reinforced glass-ceramic satisfies:
[0009]
[0010] 1.50≤X≤4.70, preferably, 1.50≤X≤4.00, more preferably, 1.50≤X≤3.60;
[0011] Wherein, CS_20 is the compressive stress value at a depth of 20 μm from the main surface of the strengthened glass-ceramic, in MPa;
[0012] CS_30 is the compressive stress value at a depth of 30 μm from the main surface of the strengthened glass-ceramic, in MPa;
[0013] CS_50 is the compressive stress value at a depth of 50 μm from the main surface of the strengthened glass-ceramic, in MPa;
[0014] DOL_0 is the depth of the compressive stress layer of the strengthened glass-ceramic, in μm;
[0015] DOL_K is K + Diffusion depth, in μm;
[0016] In formula X, the data is substituted according to the above unit requirements to perform calculations and obtain calculation results. The units do not participate in the calculations.
[0017] In the present application, by using zinc aluminum spinel-magnesium aluminum spinel solid solution as the main crystalline phase of glass ceramics, high intrinsic strength (or also known as inherent strength) can be given to glass ceramics. At the same time, the present application makes the stress at different depths of the surface of the reinforced glass ceramics whose main crystalline phase is zinc aluminum spinel-magnesium aluminum spinel solid solution, the K ion diffusion depth (or also known as K ion exchange (layer) depth) and the depth of the compressive stress layer meet the requirements of formula X, so that the surface of the reinforced glass ceramics with high intrinsic strength has a specific stress distribution structure, thereby making the reinforced glass ceramics have excellent scratch resistance. The reinforced glass ceramics are applied to electronic devices, such as mobile phones, smart watches and other electronic devices, which is beneficial to improve the service life and user experience of electronic devices. In the present application, (Zn, Mg) Al2O4 is used to represent zinc aluminum spinel-magnesium aluminum spinel solid solution.
[0018] As an optional embodiment, the reinforced glass ceramic is in plate shape; the thickness t of the reinforced glass ceramic is 0.30 mm to 2.00 mm, preferably, the thickness t is 0.35 mm to 1.50 mm, more preferably, the thickness t is 0.40 mm to 1.00 mm; and / or, the reinforced glass ceramic is 2D, 2.5D, 3D or special-shaped. At present, electronic devices are beginning to pursue thinness and lightness. When the thickness is too large, on the one hand, it will increase the weight, and on the other hand, it will cause the optical effect to deteriorate, which is not conducive to achieving high transparency.
[0019] As an optional embodiment, the reinforced glass-ceramic satisfies:
[0020] 70.00MPa≤CS_20≤250.00MPa, preferably, 75.00MPa≤CS_20≤245.00MPa, more preferably, 80.00MPa≤CS_20≤240.00MPa; and / or,
[0021] 60.00MPa≤CS_30≤240.00MPa, preferably, 65.00MPa≤CS_30≤230.00MPa, more preferably, 70.00MPa≤CS_30≤221.00MPa; and / or,
[0022] 50.00MPa≤CS_50≤210.00MPa, preferably, 55.00MPa≤CS_50≤200.00MPa, more preferably, 59.00MPa≤CS_50≤185.00MPa; and / or,
[0023] 5.00 μm≤DOL_K≤25.00 μm, preferably, 7.00 μm≤DOL_K≤23.00 μm, more preferably, 9.00 μm≤DOL_K≤21.00 μm; and / or
[0024] 0.17t≤DOL_0≤0.25t, preferably, 0.19t≤DOL_0≤0.25t, t is the thickness of the reinforced glass-ceramic; and / or,
[0025] 65.00μm≤DOL_0≤240.00μm, preferably, 70.00μm≤DOL_0≤225.00μm, more preferably, 75.00μm≤DOL_0≤215.00μm. By making the reinforced glass ceramic meet the appropriate stress structure, it is beneficial to obtain a reinforced glass ceramic product with a higher stress level, and then it is beneficial to play the role of the stress structure in improving the mechanical strength performance, ensuring that the reinforced glass ceramic meets excellent damage resistance and excellent scratch resistance.
[0026] As an optional embodiment, the reinforced glass-ceramic satisfies:
[0027] CS_20 is 104.13 MPa, 83.36 MPa, 90.30 MPa, 190.30 MPa, 203.57 MPa, 101.89 MPa, 80.76 MPa, 111.28 MPa, 122.29 MPa, 142.68 MPa, 111.31 MPa, 162.64 MPa, 172.84 MPa, 238.66 MPa or 131.91 MPa; and / or,
[0028] CS_30 is 95.34 MPa, 76.40 MPa, 78.38 MPa, 168.38 MPa, 187.61 MPa, 93.58 MPa, 73.53 MPa, 99.60 MPa, 110.58 MPa, 116.61 MPa, 103.81 MPa, 149.28 MPa, 149.98 MPa, 220.19 MPa or 124.52 MPa; and / or,
[0029] CS_50 is 78.00 MPa, 62.67 MPa, 69.80 MPa, 99.80 MPa, 156.09 MPa, 77.19 MPa, 59.24 MPa, 79.80 MPa, 87.68 MPa, 66.34 MPa, 88.96 MPa, 123.29 MPa, 124.92 MPa, 184.10 MPa or 109.86 MPa; and / or,
[0030] DOL_K is 12.20μm, 10.40μm, 9.60μm, 14.10μm, 13.30μm, 12.80μm, 11.90μm, 11. 50μm, 12.20μm, 10.10μm, 14.20μm, 12.50μm, 12.80μm, 16.30μm or 20.30μm; and / or,
[0031] DOL_0 is 150.06μm, 151.72μm, 153.34μm, 159.04μm, 148.22μm, 156.93μm, 150.10μm, 153 .34μm, 153.68μm, 78.50μm, 181.56μm, 182.52μm, 181.75μm, 188.84μm or 214.61μm; and / or,
[0032] The value of formula X is 1.90, 1.56, 2.35, 3.24, 2.07, 1.92, 1.91, 2.27, 2.21, 3.51, 1.79, 2.02, 3.43, 2.59 or 2.18.
[0033] As an optional embodiment, the Vickers hardness of the reinforced glass-ceramic is greater than or equal to 750 kgf / mm 2 Preferably, the Vickers hardness of the reinforced glass ceramic is greater than or equal to 800 kgf / mm 2 By making the Vickers hardness of the strengthened glass ceramics greater than or equal to 750kgf / mm 2 range, which makes the strengthened glass-ceramics have high hardness and high intrinsic strength, thus ensuring its excellent mechanical properties.
[0034] As an optional embodiment, the Vickers hardness of the reinforced glass ceramic is 850 kgf / mm 2 、810kgf / mm 2 、821kgf / mm 2 、824kgf / mm 2 、806kgf / mm 2 、812kgf / mm 2 、811kgf / mm 2 、823kgf / mm 2 、804kgf / mm 2 、816kgf / mm 2 、845kgf / mm 2 、814kgf / mm 2 、816kgf / mm 2 or 840kgf / mm 2 .
[0035] As an optional embodiment, the reinforced glass ceramic is transparent in the visible light wavelength range. Preferably, when the thickness t of the reinforced glass ceramic is 0.40 mm to 1.00 mm, for light with a wavelength of 550 nm, the transmittance of the reinforced glass ceramic is ≥ 85%, preferably ≥ 89%. The reinforced glass ceramic meeting this transmittance can ensure good optical properties and good transparency, and is suitable for use in electronic device display screens that require display effects.
[0036] As an optional embodiment, the composition at the center of the reinforced glass-ceramic, measured in mole percentage of oxides, comprises:
[0037] SiO2: 40.00%~50.00%, Al2O3: 20.00%~30.00%, MgO: 3.00%~8.00%, ZnO:
[0038] 8.00%~12.00%, BaO: 0%~8.00%, CaO: 0%~8.00%, ZrO2: 3.00%~6.00%, Na2O:
[0039] 2.00% to 10.00%, Li2O: 3.00% to 12.00%, K2O: 0% to 1.00%, Y2O3: 0% to 15.00% and La2O3: 0% to 15.00%. By adjusting and controlling the content range of each oxide component, it is beneficial to ensure that the strengthened glass ceramics meet the desired crystal phase structure and at the same time ensure that the strengthened glass ceramics obtain excellent optical properties and high intrinsic strength.
[0040] As an optional embodiment, the composition at the center of the reinforced glass-ceramic, measured in mole percentage of oxides, comprises:
[0041] The molar percentage of SiO2 is 41.00% to 48.00%, preferably, the molar percentage of SiO2 is 42.00% to 47.00%; and / or,
[0042] The molar percentage of Al2O3 is 22.00% to 29.00%, preferably, the molar percentage of Al2O3 is 25.00% to 28.00%; and / or,
[0043] The molar percentage of MgO is 4.00% to 7.00%, preferably, the molar percentage of MgO is 5.00% to 6.00%; and / or,
[0044] The molar percentage of ZnO is 8.50% to 11.50%, preferably, the molar percentage of ZnO is 9.00% to 11.00%; and / or,
[0045] The molar percentage of BaO is 0.50% to 5.00%, preferably, the molar percentage of BaO is 1.00% to 4.00%; and / or,
[0046] The molar percentage of CaO is 0% to 3.00%, preferably, the molar percentage of CaO is 0% to 1.50%; and / or,
[0047] The molar percentage of ZrO2 is 3.00% to 5.00%, preferably, the molar percentage of ZrO2 is 3.10% to 4.00%; and / or,
[0048] The molar percentage of Na2O is 2.50% to 8.00%, preferably, the molar percentage of Na2O is 3.00% to 6.00%; and / or,
[0049] The molar percentage of Li2O is 3.20% to 10.00%, preferably, the molar percentage of Li2O is 3.50% to 6.00%; and / or,
[0050] The molar percentage of Y2O3 is 0% to 5.00%, preferably, the molar percentage of Y2O3 is 0% to 1.00%; and / or,
[0051] The molar percentage of La2O3 is 0% to 5.00%, and preferably, the molar percentage of La2O3 is 0% to 1.00%.
[0052] As an optional embodiment, the composition at the center of the reinforced glass-ceramic, measured in mole percentage of oxides, comprises:
[0053] The molar percentage of SiO2 is 45.31%, 45.76%, 46.29%, 45.13%, 45.85%, 46.76% or 42.52%; and / or,
[0054] The molar percentage of Al2O3 is 25.80%, 27.03%, 26.36%, 25.70%, 26.10%, 26.62% or 27.36%; and / or, the molar percentage of MgO is 5.47%, 5.52%, 5.59%, 5.45%, 5.53%, 5.64% or 5.80%; and / or,
[0055] The molar percentage of ZnO is 9.71%, 9.80%, 10.91%, 9.67%, 9.82%, 9.92%, 10.02% or 9.96%; and / or,
[0056] The molar percentage of BaO is 1.16%, 1.17%, 0% or 3.47%; and / or,
[0057] The molar percentage of CaO is 0% or 0.99%; and / or,
[0058] The molar percentage of ZrO2 is 3.39%, 3.42%, 3.46%, 3.38%, 3.43%, 3.50% or 3.48%; and / or,
[0059] The molar percentage of Na2O is 3.39%, 3.43%, 3.47%, 3.38%, 5.39%, 3.50% or 3.55%; and / or,
[0060] The molar percentage of Li2O is 5.77%, 3.87%, 3.92%, 5.75%, 3.88%, 4.91%, 3.96% or 3.86%; and / or, the molar percentage of Y2O3 is 0% or 0.19%; and / or,
[0061] The molar percentage of La2O3 is 0% or 0.19%.
[0062] As an optional embodiment, the composition at the center of the reinforced glass-ceramic includes Y2O3 and / or La2O3, and the molar percentage of Y2O3 [Y2O3] and the molar percentage of La2O3 [La2O3] satisfy the following relationship: 0% < [Y2O3] + [La2O3] ≤ 15.00%; preferably, 0% < [Y2O3] + [La2O3] ≤ 5.00%, and more preferably, 0% < [Y2O3] + [La2O3] ≤ 1.00%. On the basis of adjusting and controlling the content range of each oxide component, by adding an appropriate amount of Y2O3 and / or La2O3, the strength, hardness, stability and deformation resistance of the reinforced glass-ceramic are improved.
[0063] As an optional embodiment, the composition at the center of the reinforced glass-ceramic satisfies that the value of [Y2O3]+[La2O3] is 0% or 0.38%.
[0064] As an optional embodiment, in terms of the molar percentage of oxides, the composition of the reinforced glass ceramics: does not contain P2O5, and / or does not contain B2O3, and / or does not contain TiO2. In the composition of the reinforced glass ceramics of the present application, the addition of P2O5 is likely to affect the optical properties of the reinforced glass ceramics, the addition of B2O3 can improve the melting effect of the substrate glass, but is likely to affect the toughness and other properties of the reinforced glass ceramics, and the addition of TiO2 is likely to cause the reinforced glass ceramics to present an undesirable color. Therefore, it is preferred that the reinforced glass ceramics of the present application do not contain P2O5, B2O3, and TiO2.
[0065] As an optional embodiment, the crystallinity of the reinforced glass ceramic is 30% to 55%, preferably 40% to 55%; and / or, in the reinforced glass ceramic, the average crystal size does not exceed 20nm, preferably 1nm to 15nm, more preferably 3nm to 8nm. By making the glass ceramic meet the desired crystallinity and appropriate average grain size, it is beneficial to make the glass ceramic maintain excellent optical properties while meeting excellent mechanical strength properties and high intrinsic strength.
[0066] As an optional embodiment, the reinforced glass-ceramic, after the sand and stone scratch test, has a haze growth factor of less than 3.00, preferably less than 2.50, and more preferably less than 2.10, compared with the haze of the reinforced glass-ceramic before the sand and stone scratch test;
[0067] Among them, the sand and gravel scratch test refers to placing the reinforced glass ceramic and 1kg of silica sand in an oscillating abraser for scratch testing, the oscillation frequency of the oscillating abraser is 150 rpm, and the time of the sand and gravel scratch test is 10 minutes; the haze growth factor = (the final haze of the reinforced glass ceramic after the sand and gravel scratch test - the initial haze of the reinforced glass ceramic before the sand and gravel scratch test) / the initial haze of the reinforced glass ceramic before the sand and gravel scratch test. The smaller the haze growth factor after the scratch test, the less damage the reinforced glass ceramic suffered during the scratch test, and the better its scratch resistance.
[0068] In a second aspect, a cover glass is provided, wherein the cover glass is made of the tempered glass ceramic as described in any embodiment of the first aspect.
[0069] In a third aspect, an electronic device is provided, wherein the electronic device comprises the reinforced glass ceramic as described in any embodiment of the first aspect.
[0070] As an optional embodiment, the electronic device includes a housing assembled on the outside of the electronic device, and the housing includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0071] As an optional embodiment, the housing includes a display screen cover assembled on the front side of the electronic device, and the display screen cover includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0072] As an optional embodiment, the housing includes a back cover assembled on the back side of the electronic device, and the back cover includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0073] As an optional embodiment, the electronic device also includes a camera assembly located inside the housing, the housing includes a camera protection cover, the camera protection cover is covered on the camera assembly, and the camera protection cover includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0074] As an optional embodiment, the electronic device further includes a middle frame, and the middle frame includes the reinforced glass ceramic as described in any embodiment of the first aspect.
[0075] In some embodiments, the housing may be partially or entirely made of reinforced glass ceramics. The electronic device in the present application may be a display cover, a back cover, a camera protection cover, a middle frame, or one or more of which may be made of the reinforced glass ceramics described in any embodiment of the first aspect.
[0076] In a fourth aspect, a glass device is provided, wherein the glass device comprises the reinforced glass ceramic as described in any embodiment of the first aspect.
[0077] One or more of the above technical solutions provided by the present application have the following advantages compared with the prior art:
[0078] In the present application, by using zinc aluminum spinel-magnesium aluminum spinel solid solution as the main crystalline phase of glass ceramics, high intrinsic strength (or also called inherent strength) can be given to glass ceramics. At the same time, the present application makes the stress at different depths of the surface of the reinforced glass ceramics whose main crystalline phase is zinc aluminum spinel-magnesium aluminum spinel solid solution, the K ion diffusion depth (or also called K ion exchange (layer) depth) and the depth of the compressive stress layer meet the requirements of formula X, so that the surface of the reinforced glass ceramics with high intrinsic strength has a specific stress distribution structure, thereby making the reinforced glass ceramics have excellent scratch resistance. The reinforced glass ceramics are applied to electronic devices, such as mobile phones, smart watches and other electronic devices, which is beneficial to improve the service life and user experience of electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0079] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0080] Figure 1 Schematic diagram of the model of sand and gravel rubbing against glass-ceramic surface.
[0081] Figure 2This is a schematic diagram of the front structure of the electronic device mentioned in the implementation mode of this application.
[0082] Figure 3 This is a schematic diagram of the rear structure of the electronic device mentioned in the implementation mode of this application.
[0083] Figure 4 The structure of the electronic device mentioned in the embodiment of this application is schematically shown. Figure 1 .
[0084] Figure 5 This is a comparison chart of the XRD spectra of the glass ceramic and the reinforced glass ceramic provided in Example 1 of the present application.
[0085] Figure 6 This is a comparison chart of the transmittance curves of the glass ceramic and the reinforced glass ceramic provided in Example 1 of the present application. The "before strengthening" curve in the figure refers to the transmittance curve of the glass ceramic, and the "after strengthening" curve refers to the transmittance curve of the reinforced glass ceramic.
[0086] Figure 7 The scratch point micrographs of the reinforced glass-ceramics provided in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 of the present application after the sand and gravel scratch test, wherein the black dots are scratch points, wherein a is the test result of Example 1, b is the test result of Example 2, c is the test result of Comparative Example 1, and d is the test result of Comparative Example 2.
[0087] Figure 8 The structure of the electronic device mentioned in the embodiment of this application is schematically shown. Figure 2 .
[0088] Fig. 9 This is a physical comparison diagram of the reinforced glass ceramics of Example 4 and Comparative Example 2 of the present application after being subjected to a sand and stone scratch test, a is Example 4, and b is Comparative Example 2.
[0089] Figure numerals: 1-housing; 11-display screen cover; 12-back cover; 13-camera protection cover; 2-camera assembly; 3-middle frame; 4-display module. DETAILED DESCRIPTION
[0090] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0091] The endpoints and any values of the ranges disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all refer to including or not including (or may have or may not have). "And / or" as referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0092] Explanation of terms and test methods:
[0093] In the present application, glass ceramics are a type of solid composite material that is prepared by targeted controlled heat treatment of substrate glass and contains both a glass phase and a crystal phase (also called microcrystalline phase, crystal phase, or crystalline phase). Glass ceramics are also called microcrystalline glass or crystallized glass.
[0094] In the present application, the strengthened glass ceramic refers to a solid composite material obtained by chemically strengthening the glass ceramic. It should be understood that during the chemical strengthening treatment, the alkali metal ions (such as potassium ions or sodium ions) with large ionic radius in the molten salt bath (or also called molten salt bath) will replace the alkali metal ions (such as sodium ions or lithium ions) with small ionic radius in the glass ceramic, thereby generating an exchange ion volume difference and generating compressive stress (or also called compressive stress) on the surface of the glass ceramic.
[0095] In the present application, substrate glass refers to glass that has not been subjected to nucleation treatment, crystallization treatment, and strengthening treatment, or is also called basic glass.
[0096] In the present application, the composition at the center of the strengthened glass-ceramic refers to the composition at the center of the depth or thickness of the strengthened glass-ceramic or near the center of the depth or thickness, that is, the composition of the region in the strengthened glass-ceramic where ion exchange has not been performed. It should be understood that the composition at the center of the strengthened glass-ceramic is the same or substantially the same as the composition of the glass-ceramic used to prepare the strengthened glass-ceramic but has not yet been chemically strengthened.
[0097] In the present application, the visible light wavelength range refers to 360nm to 740nm.
[0098] In the present application, haze is the percentage of the transmitted light intensity that deviates from the incident light by more than 2.5° to the total transmitted light intensity.
[0099] In the present application, fogging refers to a semi-transparent state, which is between transparency and devitrification, due to large crystals or phase separation in the glass ceramic.
[0100] In the present application, devitrification means that due to large crystals or phase separation in the glass ceramic, the transparent property of the glass is completely lost, and any image on the back cannot be seen through the glass.
[0101] In the present application, the main crystalline phase (or also referred to as the main crystalline phase) refers to a crystalline phase having a higher weight content (or also referred to as weight percentage, mass percentage) than other crystalline phases present in the glass-ceramic.
[0102] In the present application, crystallinity refers to the percentage of the total mass of the crystalline phase or crystals in the glass-ceramic to the mass of the glass-ceramic, or is also referred to as the total content of the crystalline phase in the glass-ceramic.
[0103] In the present application, the main surface refers to the surface with the largest surface area, such as the upper surface or the lower surface of a horizontally placed glass ceramic sheet.
[0104] In the present application, when light of a certain wavelength is irradiated onto the main surface of the glass ceramic, the light will be reflected, absorbed and transmitted, wherein the ratio of the intensity of the transmitted part to the intensity of the incident light is the transmittance.
[0105] In the present application, CS_20, CS_30, and CS_50 refer to the compressive stress values at a depth of 20 μm, 30 μm, and 50 μm from the main surface of the self-strengthened glass-ceramic, respectively, in MPa, and are obtained by testing with an SLP-2000 stress meter (or also known as a scattered light photoelastic stress meter).
[0106] In this application, DOL_0 refers to the depth of the compressive stress layer, or the depth of the compressive stress layer, specifically the distance from any main surface of the strengthened glass-ceramic to the position close to the surface where the compressive stress is zero, obtained by testing with an SLP-2000 stress meter.
[0107] In this application, the test method of the aforementioned stress performance is as follows: when using the SLP-2000 stress meter to test the CS_20, CS_30, CS_50, and DOL_0 of the reinforced glass ceramics, the relevant parameters of the stress meter are set as follows: the wavelength of the light source is 518nm, SOC=25.5 (nm / cm) / MPa, the refractive index=1.60, and the exposure time is 300μsec. The special refractive liquid is dripped on the stress meter, and then the reinforced glass ceramic product is wiped clean and placed on the test path to test its value. The refractive index of the refractive liquid used by SLP-2000 is 1.51.
[0108] In this application, SOC, or photoelastic coefficient, mainly refers to the phenomenon of birefringence caused by anisotropy in transparent materials after being subjected to force. The value of residual stress inside the material can be obtained by measuring the photoelastic coefficient and birefringence.
[0109] In this application, DOL_K refers to K + Diffusion depth, or K +Diffusion layer depth, also known as K + The exchange (layer) depth refers to the depth from any main surface of the strengthened glass-ceramic to the K measured by EPMA. + The depth at which the slope value of the concentration distribution curve (or also called the K element concentration distribution curve) is equal to 0.000 for the first time is obtained by Shimadzu electron probe EPMA-1720HT test. In this application, the K from the main surface to the inside of the strengthened glass-ceramic measured by EPMA is + In the concentration distribution curve, K + After ion exchange, it diffuses into the surface of glass ceramics, and with the increase of depth, K + The amount in the glass ceramic decreases, and finally reaches the depth where the slope of the curve is equal to 0.000 for the first time. + No longer spread inside.
[0110] Electron probe X-ray microanalysis (EPMA) test: Take the tested strengthened glass ceramic sample, mechanically grind one side perpendicular to the glass surface, remove the strengthening layer (wear removal is more than 500μm), obtain a cross-section sample, perform 30nm carbon spraying on the ground cross section, focus the electron beam along the ground cross section to select a straight line in the thickness direction for line scanning, and obtain the element composition and element concentration distribution in the thickness direction. The electron probe X-ray microanalysis instrument used in this application is Shimadzu's EPMA-1720HT, with an acceleration voltage of 15kV, a probe current of 100nA, a beam size of MIN, a step interval of 1μm, and a time of 1s / point; spectroscopic crystal RAP (Na Kα ray), spectroscopic crystal PET (K Kα ray); test elements: Na, K.
[0111] In this application, scratches refer to permanent scratches left by objects such as sand and stone after rubbing against the surface of glass ceramics.
[0112] In the present application, Vickers hardness refers to a standard for expressing the hardness of materials proposed by Robert L. Smith and George E. Sandland of the United Kingdom at Vickers Ltd in 1921.
[0113] In this application, the test method of Vickers hardness is as follows: the reinforced glass ceramic is made into a small piece of 50mm×50mm×0.70mm or φ46mm×0.70mm, and a glass sample with a clean surface and no visible scratches, pits, cracks and other damage is selected as a test sample / sample, and then the Vickers hardness is measured using a Vickers hardness tester. The Vickers hardness tester used in the test of this application is a digital display small load Vickers hardness tester model VTD405 of Beijing Kewei Technology Co., Ltd. Test conditions: load 300gf, load time 10s, the effectiveness of the indentation complies with the "GB / T37900-2019 Ultra-thin glass hardness and fracture toughness test method small load Vickers hardness indentation method" standard. Select 3 different positions on the surface of the same test sample / sample for measurement, and take the average of the 3 measurement results, which is recorded as the Vickers hardness result of the test sample / sample.
[0114] In the present application, the thickness of the glass ceramic is obtained by micrometer testing. It should be understood that in the thickness direction, the degree of ion exchange changes gradually from the surface to the center, and the overall Na-K and / or Li-Na exchange amount increment (mass) generally does not exceed 1.5% of the total mass of the sample, so the expansion effect in the thickness direction is extremely slight, and it can be approximately considered that the thickness has basically not changed. That is, before and after chemical strengthening, the thickness of the glass ceramic changes very little, which can be basically ignored, and the thickness of the glass ceramic is basically the same as the thickness of the strengthened glass ceramic obtained therefrom.
[0115] In the present application, the density test adopts the electronic density balance SD-200L of Japan ALFAMIRAGE to test the density of glass ceramics.
[0116] In this application, the size specifications of the glass ceramic sheet are tested using a two-dimensional measuring machine (instrument model: MiyuMY-YXCL-4030).
[0117] In this application, the crystal phase composition, crystallinity and average crystal size of the glass ceramics were confirmed by XRD testing, as follows:
[0118] (1) XRD test: The glass ceramic or reinforced glass ceramic of the present application is crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample is tested using an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The X-ray diffractometer used in the present application is Shimadzu XRD-6100, the target material is copper, 2θ=10°-80°, the scanning speed is 2° / min, the operating voltage is 40 kV, and the operating current is 30 mA.
[0119] (2) Determination of crystalline phase: XRD diffraction data were analyzed using Jade software (JADE Standard 8.6) to determine the crystalline phase in the sample.
[0120] (3) Determination of crystallinity: The XRD test results (RAW format) were imported into the Jade software for fitting, and the crystallinity of the sample was determined by calculating the formula (diffraction peak intensity / total intensity) × 100%.
[0121] (4) Determination of average crystal size: The average crystal size (or also called average grain size) of the sample can be calculated using the result data obtained from the XRD test according to the Scherrer formula D = Kλ / (βcosθ). Wherein, λ is the wavelength of the X-ray, λ = 0.154056nm, β is the half-height width of the diffraction peak, K = 0.89, and θ is the Bragg diffraction angle. Specifically, the RAW format file output by the XRD instrument is curve fitted in the Jade software, and Jade outputs a fitting report. According to the angle 2θ value and Peak FWHM value corresponding to each diffraction peak in the fitting report, the Peak FWHM value is converted into radians: β = (FWHM / 180×3.14), and the grain size of each diffraction peak is calculated by the Scherrer formula D = Kλ / (βcosθ) and then averaged to obtain the average crystal size in the sample.
[0122] In this application, with reference to the national standard "GB / T7962.12-2010 Test Method for Colorless Optical Glass Part 12: Spectral Transmittance", a haze meter is used to test the transmittance and haze of the glass ceramics of this application. Specifically, a haze meter is used to test the transmittance and haze of 5 glass ceramics of the same batch to light of different wavelengths. The average value of the haze measured by the 5 glass ceramics is taken as the haze result of the glass ceramics. The average value of the transmittance measured by the 5 glass ceramics under 550nm wavelength light is taken as the transmittance result of the glass ceramics under 550nm wavelength light. The haze meter used in the test of this application is a Japanese Konica Minolta spectrophotometer CM-3600A, the light receiving optical system is transmission, the spectral mode is a plane refractive grating, the wavelength range is 360nm-740nm, the wavelength spacing is 10nm, the illumination light source is a pulse xenon lamp × 4, the ambient temperature of the instrument is 24°C, and the air humidity is 40%.
[0123] In this application, the American Taber oscillating abrasion tester is used to perform the sand and stone scratch test on the reinforced glass ceramics, and after the sand and stone scratch test, the haze growth multiple of the reinforced glass ceramics is tested. The specific test process is as follows: take the reinforced glass ceramic sample to be tested, the surface is clean and there is no visible scratches, pits and cracks and other damages, measure its initial haze, and then stick the reinforced glass ceramic sample to be tested on the bottom plate with tape, and put the bottom plate with the sample stuck in the oscillating abrasion tester, so that the reinforced glass ceramic sample faces up, and cover the reinforced glass ceramic sample with silica sand, the weight of the silica sand is 1kg, the particle size is less than 2.5mm, and the oscillation frequency of the oscillating abrasion tester is set to 150 rpm, and the reinforced glass ceramic sample is subjected to the sand and stone scratch test, and the test time is 10min. After the test, take out the reinforced glass ceramic sample, clean it and test its final haze after the sand and stone scratch test. Haze growth factor = (final haze of the reinforced glass ceramic after the sand and stone scratch test - initial haze of the reinforced glass ceramic before the sand and stone scratch test) / initial haze of the reinforced glass ceramic before the sand and stone scratch test.
[0124] In daily use, the cover glass on the surface of electronic devices, in addition to facing destructive damage caused by falling, impact, squeezing, etc., will also face the problem of scratches from objects such as dust or dirt. Dust or dirt scratches are also called abrasive wear. When a solid surface comes into contact with dust or dirt, the protruding parts contact each other, and are subjected to great pressure and produce plastic deformation and then adhesion. The adhesion part causes the side of the weaker material to be sheared due to friction and sliding, and is adhered to the side with stronger hardness. Scratches, or also called damage points, are formed on the surface of the weaker material, resulting in scratches, such as Figure 1 Scratches will leave scratches, resulting in a particularly rough feel, and when the scratches are severe, they will directly affect the display effect of the screen.
[0125] Without being bound by any theory, when the size of dust or dirt (or sand and gravel) is less than 500μm, the distance of the scratches produced after scratching is very small, and smaller scratches can remove materials, thereby causing greater damage to the surface. Material removal is related to the interaction strength of the scratches separating adjacent modules, resulting in the removal of glass materials. When the scratch distance is 1-2μm, larger-sized transverse cracks propagate to the surface, resulting in brittle peeling of the material. When the scratch distance is 4-10μm, the material is mainly removed in a tough manner. Glass brittleness is related to surface microcracks and air bubbles. Increasing the stress on the surface of the glass to 50μm and giving the glass surface a specific stress distribution structure can reduce the above problems, because the specific stress distribution structure can reduce the crack propagation ability, inhibit the expansion of cracks, and slow down the attenuation of elastic recovery. Enhanced toughness and elastic recovery are obtained by increasing the stiffness and strength of the material. Elastic recovery refers to the degree to which the material recovers to the level before the force is applied after the external force is eliminated. It is related to the elastic modulus, strength, deformation, fracture and other properties of the material, or crystallization inside the glass.
[0126] In theory, the precipitation of high-hardness crystals in the glass-ceramic material, for example, spinel crystals belonging to the cubic system, is beneficial to improving the scratch resistance of the glass-ceramic material. Specifically, the chemical formula of the spinel crystal is AB2O4, wherein A is a divalent metal ion such as Zn, Fe or Mg with tetrahedral coordination, and B is an Al, Cr or Fe metal ion with octahedral coordination. For example, Figure 1 The zinc aluminum spinel-magnesium aluminum spinel solid solution ((Zn,Mg)Al2O4) is shown. Common spinel crystals include magnesium aluminum spinel (MgAl2O4, also known as magnesium spinel) crystals and zinc aluminum spinel (ZnAl2O4, also known as zinc spinel) crystals. Since Al-O, Mg-O, and Zn-O can form strong ionic bonds, their structure is strong, hardness is high, and chemical properties are stable. The Mohs hardness level of spinel crystals is basically between 7 and 8, close to 8. The strength of silicon dioxide yields to spinel, so common dust and dust are usually not easy to scratch glass ceramic materials with spinel crystals as the main crystal phase. Therefore, by controllably precipitating zinc aluminum spinel crystals and / or magnesium aluminum spinel crystals and / or zinc aluminum spinel-magnesium aluminum spinel solid solution ((Zn,Mg)Al2O4) in the glass, it is theoretically possible to obtain spinel glass ceramics with good mechanical properties and good scratch resistance.
[0127] However, the present application further discovered that glass ceramic materials with spinel crystals as the main crystal phase do not necessarily achieve excellent scratch resistance after strengthening. The scratch resistance of strengthened glass ceramic materials is closely related to the crystal phase composition of the strengthened glass ceramics and the surface stress distribution structure.
[0128] To this end, in order to make the reinforced glass-ceramics with spinel crystals as the main crystal phase obtain excellent scratch resistance, the present application further studies the crystal phase composition and surface stress distribution structure of the reinforced glass-ceramics. It is found that the stress distribution structure of the surface of the reinforced glass-ceramics to a depth of 50μm is crucial to improving the scratch resistance of the reinforced glass-ceramics. The greater the external force applied to the surface, the more drastically the elastic recovery decreases until the reinforced glass-ceramics are left with permanent damage, and the surface stress structure of the reinforced glass-ceramics counteracts the external force applied to the surface, which can slow down the attenuation of the elastic recovery and enhance the scratch resistance of the reinforced glass-ceramics. That is, when the stress distribution structure on the surface of the reinforced glass-ceramics meets specific requirements, it can ensure that the reinforced glass-ceramics obtain excellent scratch resistance.
[0129] In view of this, the present application provides a strengthened glass-ceramic material that satisfies a specific crystal phase composition and a specific stress distribution structure on the surface. The strengthened glass-ceramic is used as the display screen cover glass of an electronic device. Even if the scratch-resistant coating on its surface is worn off, it can still maintain excellent scratch resistance.
[0130] In some embodiments of the present application, a reinforced glass ceramic is provided, wherein the reinforced glass ceramic comprises a main crystalline phase of zinc aluminum spinel-magnesium aluminum spinel solid solution and a secondary crystalline phase of zirconium oxide;
[0131] The reinforced glass-ceramic has a compressive stress layer on the surface and tensile stress inside; the reinforced glass-ceramic satisfies:
[0132]
[0133] 1.50≤X≤4.70, preferably, 1.50≤X≤4.00, more preferably, 1.50≤X≤3.60;
[0134] Wherein, CS_20 is the compressive stress value at a depth of 20 μm from the main surface of the strengthened glass-ceramic, measured by SLP_2000, in MPa;
[0135] CS_30 is the compressive stress value at a depth of 30 μm from the main surface of the strengthened glass-ceramic, measured by SLP_2000, in MPa;
[0136] CS_50 is the compressive stress value at a depth of 50 μm from the main surface of the strengthened glass-ceramic, measured by SLP_2000, in MPa;
[0137] DOL_0 is the depth of the compressive stress layer of the strengthened glass-ceramics, measured by SLP_2000, in μm;
[0138] DOL_K is K +Diffusion depth, measured by EPMA, in μm;
[0139] In formula X, the data is substituted according to the above unit requirements to perform calculations and obtain calculation results. The units do not participate in the calculations.
[0140] In the present application, by using zinc aluminum spinel-magnesium aluminum spinel solid solution as the main crystalline phase of glass ceramics, high intrinsic strength (or also known as inherent strength) can be given to glass ceramics. At the same time, the present application satisfies the requirements of formula X by making the stress at different depths of the surface of the reinforced glass ceramics whose main crystalline phase is zinc aluminum spinel-magnesium aluminum spinel solid solution, the K ion diffusion depth (or also known as K ion exchange depth) and the depth of the compressive stress layer, so that the surface of the reinforced glass ceramics with high intrinsic strength has a specific stress distribution structure, thereby making the reinforced glass ceramics have excellent scratch resistance. The reinforced glass ceramics are applied to electronic devices, such as mobile phones, smart watches and other electronic devices, which is beneficial to improve the service life and user experience of electronic devices. In the present application, (Zn, Mg) Al2O4 is used to represent zinc aluminum spinel-magnesium aluminum spinel solid solution (or also known as zinc spinel-magnesium spinel solid solution, zinc magnesium spinel solid solution).
[0141] In some embodiments, the value of the formula X may satisfy: 1.50≤X≤3.55, 1.75≤X≤3.45, 1.90≤X≤3.25, or 2.05≤X≤2.60. In some embodiments, the value of formula X can be 1.50, 1.55, 1.60, 1.65, 1.70, 1.75, 1.85, 1.90, 1.95, 2.00, 2.05, 2.10, 2.15, 2.20, 2.25, 2.30, 2.35, 2.40, 2.45, 2.50, 2.55, 2.60, 2.65, 2.70, 2.75, 2.80, 2.85, 2.90, 2.95, 3.00, 3.05, 3.10, 3.15, 3.20, 3.25, 3.30, 3.35, 3.40, 3.45, 3.50, 3.55, 3.60, 3.70, 3.80, 3.90, 4.10, 4.20, 4.30, 4.40, 4.55 .65, 3.70, 3.75, 3.80, 3.85, 3.90, 3.95, 4.00, 4.05, 4.10, 4.15, 4.20, 4.25, 4.30, 4.35, 4.40, 4.45, 4.50, 4.55, 4.60, 4.65, 4.70, 1.56, 3.24, 2.07, 1.92, 1.91, 2.27, 2.21, 3.51, 1.79, 2.02, 3.43, 2.59 or 2.18, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0142] In some embodiments of the present application, the strengthened glass-ceramic satisfies: 70.00 MPa≤CS_20≤250.00 MPa, preferably, 75.00 MPa≤CS_20≤245.00 MPa, and more preferably, 80.00 MPa≤CS_20≤240.00 MPa.
[0143] In some embodiments, the CS_20 of the strengthened glass-ceramic may satisfy: 90.00MPa≤CS_20≤239.00MPa, 101.00MPa≤CS_20≤204.00MPa, 111.00MPa≤CS_20≤191.00MPa, 122.00MPa≤CS_20≤
[0144] 173.00MPa or 131.00MPa≤CS_20≤163.00MPa. In some embodiments, the CS_20 of the strengthened glass-ceramic can be: 70.00MPa, 75.00MPa, 80.00MPa, 85.00MPa, 90.00MPa, 95.00MPa, 100.00MPa, 105.00MPa, 110.00MPa, 115.00MPa, 120.00MPa, 125.00MPa, 130.00MPa, 135.00MPa, 140.00MPa, 145.00MPa, 150.00MPa, 155.00MPa, 160.00MPa, 165.00MPa, 170.00MPa, 175.00MPa,
[0145] 180.00MPa, 185.00MPa, 190.00MPa, 195.00MPa, 200.00MPa, 205.00MPa, 210.00MPa,
[0146] 215.00MPa, 220.00MPa, 225.00MPa, 230.00MPa, 240.00MPa, 250.00MPa, 104.13MPa,
[0147] 83.36MPa, 90.30MPa, 190.30MPa, 203.57MPa, 101.89MPa, 80.76MPa, 111.28MPa, 122.29MPa, 142.68MPa, 111.31MPa, 162.64MPa, 172.84MPa, 238.66MPa or 131.91MPa, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0148] In some embodiments of the present application, the strengthened glass-ceramic satisfies: 60.00 MPa≤CS_30≤240.00 MPa, preferably, 65.00 MPa≤CS_30≤230.00 MPa, and more preferably, 70.00 MPa≤CS_30≤221.00 MPa.
[0149] In some embodiments, the CS_30 of the strengthened glass-ceramic may satisfy: 78.00 MPa≤CS_30≤221.00 MPa, 93.00 MPa≤CS_30≤188.00 MPa, 99.00 MPa≤CS_30≤169.00 MPa, 110.00 MPa≤CS_30≤145.00 MPa, or 116.00 MPa≤CS_30≤125.00 MPa. In some embodiments, the CS_30 of the strengthened glass-ceramic can be: 60.00MPa, 65.00MPa, 70.00MPa, 75.00MPa, 80.00MPa, 85.00MPa, 90.00MPa, 95.00MPa, 100.00MPa, 105.00MPa, 110.00MPa, 115.00MPa, 120.00MPa, 125.00MPa, 130.00MPa, 135.00MPa, 140.00MPa, 145.00MPa, 150.00MPa, 155.00MPa, 160.00MPa, 165.00MPa,
[0150] 170.00MPa, 175.00MPa, 180.00MPa, 185.00MPa, 190.00MPa, 195.00MPa, 200.00MPa,
[0151] 205.00MPa, 210.00MPa, 215.00MPa, 220.00MPa, 225.00MPa, 230.00MPa, 235.00MPa,
[0152] 240.00MPa, 95.34MPa, 76.40MPa, 78.38MPa, 168.38MPa, 187.61MPa, 93.58MPa, 73.53MPa,
[0153] 99.60MPa, 110.58MPa, 116.61MPa, 103.81MPa, 149.28MPa, 149.98MPa, 220.19MPa or 124.52MPa, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the performance required by the present application can be obtained.
[0154] In some embodiments of the present application, the strengthened glass-ceramic satisfies: 50.00 MPa≤CS_50≤210.00 MPa, preferably, 55.00 MPa≤CS_50≤200.00 MPa, and more preferably, 59.00 MPa≤CS_50≤185.00 MPa.
[0155] In some embodiments, the CS_50 of the strengthened glass-ceramic may satisfy: 62.00 MPa≤CS_50≤184.00 MPa, 66.00 MPa≤CS_50≤160.00 MPa, 69.00 MPa≤CS_50≤130.00 MPa, 75.00 MPa≤CS_50≤110.00 MPa, or 85.00 MPa≤CS_50≤100.00 MPa. In some embodiments, the CS_50 of the strengthened glass-ceramic can be: 50.00MPa, 55.00MPa, 60.00MPa, 65.00MPa, 70.00MPa, 75.00MPa, 80.00MPa, 85.00MPa, 90.00MPa, 95.00MPa, 100.00MPa, 105.00MPa, 110.00MPa, 115.00MPa, 120.00MPa, 125.00MPa,
[0156] 130.00MPa, 135.00MPa, 140.00MPa, 145.00MPa, 150.00MPa, 155.00MPa, 160.00MPa,
[0157] 165.00MPa, 170.00MPa, 175.00MPa, 180.00MPa, 185.00MPa, 190.00MPa, 195.00MPa, 200 .00MPa, 205.00MPa, 210.00MPa, 78.00MPa, 62.67MPa, 69.80MPa, 99.80MPa, 156.09MPa, 7 7.19MPa, 59.24MPa, 79.80MPa, 87.68MPa, 66.34MPa, 88.96MPa, 123.29MPa, 124.92MPa, 184.10MPa or 109.86MPa, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0158] In some embodiments of the present application, the strengthened glass-ceramic satisfies: 5.00 μm ≤ DOL_K ≤ 25.00 μm, preferably, 7.00 μm ≤ DOL_K ≤ 23.00 μm, and more preferably, 9.00 μm ≤ DOL_K ≤ 21.00 μm.
[0159] In some embodiments, the DOL_K of the strengthened glass-ceramic may satisfy: 10.00 μm≤DOL_K≤17.00 μm, 11.00 μm≤DOL_K≤15.00 μm, 12.00 μm≤DOL_K≤14.00 μm, or 12.00 μm≤DOL_K≤13.00 μm. In some embodiments, the DOL_K of the strengthened glass-ceramic may be 5.00 μm, 5.50 μm, 6.00 μm, 6.50 μm, 7.00 μm, 7.50 μm, 8.00 μm, 8.50 μm, 9.00 μm, 9.50 μm, 10.00 μm, 10.50 μm, 11.00 μm, 11.50 μm, 12.00 μm, 12.50 μm, 13.00 μm, 13.50 μm, 14.00 μm, 14.50 μm, 15.00 μm, 15.50 μm, 16.00 μm, 16.50 μm,
[0160] 17.00μm, 17.50μm, 18.00μm, 18.50μm, 19.00μm, 19.50μm, 20.00μm, 20.50μm, 21.00μm, 21.50μm, 22.00μm, 22.50μm, 23.00μm, 23.50μm, 24.00μm, 24.50μm, 25.00μm, 12.20μm,
[0161] 10.40μm, 9.60μm, 14.10μm, 13.30μm, 12.80μm, 11.90μm, 11.50μm, 12.20μm, 10.10μm, 14.20μm, 12.50μm, 12.80μm, 16.30μm or 20.30μm, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0162] In some embodiments of the present application, the reinforced glass-ceramic satisfies: 0.17t≤DOL_0≤0.25t, preferably, 0.19t≤DOL_0≤0.25t, where t is the thickness of the reinforced glass-ceramic. In some embodiments, the DOL_0 of the reinforced glass-ceramic can be 0.17t, 0.18t, 0.19t, 0.20t, 0.21t, 0.22t, 0.23t, 0.24t or 0.25t, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0163] In some embodiments of the present application, the strengthened glass-ceramic satisfies: 65.00 μm≤DOL_0≤240.00 μm, preferably, 70.00 μm≤DOL_0≤225.00 μm, and more preferably, 75.00 μm≤DOL_0≤215.00 μm.
[0164] In some embodiments, the DOL_0 of the strengthened glass-ceramic may satisfy: 78.00 μm≤DOL_0≤215.00 μm, 148.00 μm≤DOL_0≤189.00 μm, 150.00 μm≤DOL_0≤190.00 μm, 153.00 μm≤DOL_0≤183.00 μm, or 153.00 μm≤DOL_0≤160.00 μm. In some embodiments, the DOL_0 of the strengthened glass-ceramic may be: 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 105 μm, 110 μm, 115 μm, 120 μm, 125 μm, 130 μm, 135 μm, 140 μm, 145 μm, 150 μm, 155 μm, 160 μm, 165 μm, 170 μm, 175 μm, 180 μm,
[0165] 185μm, 190μm, 195μm, 200μm, 205μm, 210μm, 215μm, 220μm, 225μm, 230μm, 235μm, 2 40μm, 150.06μm, 151.72μm, 153.34μm, 159.04μm, 148.22μm, 156.93μm, 150.10μm,
[0166] 153.34 μm, 153.68 μm, 78.50 μm, 181.56 μm, 182.52 μm, 181.75 μm, 188.84 μm or 214.61 μm, or it can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the performance required by the present application can be obtained.
[0167] In the present application, by making the reinforced glass-ceramics meet the appropriate stress structure, it is beneficial to obtain reinforced glass-ceramic products with a higher stress level, and then it is beneficial to give play to the improvement effect of the stress structure on the mechanical strength performance, ensuring that the reinforced glass-ceramics meet excellent damage resistance and excellent scratch resistance.
[0168] Those skilled in the art can select the thickness of glass ceramics or reinforced glass ceramics according to demand. In some embodiments of the present application, the glass ceramics or reinforced glass ceramics are plate-shaped; the thickness t of the glass ceramics or reinforced glass ceramics is 0.30mm~2.00mm, preferably, the thickness t is 0.35mm~1.50mm, and more preferably, the thickness t is 0.40mm~1.00mm. Exemplarily, the thickness t of the glass ceramics or reinforced glass ceramics can be 0.30mm~1.50mm, 0.30mm~1.00mm or 0.40~0.80mm, 0.80mm~1.30mm or 0.70~1.00mm. At present, electronic devices are beginning to pursue lightness and thinness. When the thickness is too large, on the one hand, it will increase the weight, and on the other hand, it will cause the optical effect to deteriorate, which is not conducive to achieving high transparency.
[0169] In some embodiments of the present application, the glass ceramic or reinforced glass ceramic is 2D, 2.5D, 3D or special-shaped, that is, the glass ceramic can be a 2D, 2.5D, 3D or special-shaped product, and the reinforced glass ceramic can also be a 2D, 2.5D, 3D or special-shaped product; and / or, the glass ceramic or reinforced glass ceramic is of equal thickness or unequal thickness. Those skilled in the art can make a choice according to demand. Here, "unequal thickness" means that the glass ceramic or reinforced glass ceramic contains at least two parts with different thicknesses.
[0170] In the present application, the spinel solid solution (Zn,Mg)Al2O4 as the main crystalline phase and the tetragonal ZrO2 secondary crystalline phase do not contain alkali metal ions, so they do not participate in the ion exchange during the chemical strengthening process. Based on this, the crystal phase structure of the strengthened glass ceramics obtained by chemical strengthening in the present application is basically the same as the glass ceramics used for chemical strengthening. That is, the crystal phase content, crystal composition, crystal size and other crystal phase structure characteristics of the strengthened glass ceramics obtained by the chemical strengthening process in the present application are basically the same as the glass ceramics used for chemical strengthening in the preparation of the strengthened glass ceramics in the present application. Figure 5 As shown in FIG. 1 , in Example 1, the XRD patterns of the glass ceramic before chemical strengthening and the strengthened glass ceramic after chemical strengthening are substantially the same. Figure 6 As shown, in the present application, the transmittance of the glass ceramics before and after chemical strengthening is basically the same as the transmittance of the strengthened glass ceramics. That is to say, in the present application, by using glass ceramics with high transmittance, chemical strengthening treatment can be performed to obtain strengthened glass ceramic products with the same excellent transmittance.
[0171] It should be understood that the stress structure generated by the chemical strengthening process can appropriately improve the mechanical properties of glass products. Therefore, in the present application, after the glass ceramics are chemically strengthened to obtain strengthened glass ceramics, their mechanical properties such as Young's modulus and Vickers hardness will not decrease.
[0172] In some embodiments of the present application, the Vickers hardness of the reinforced glass-ceramic is greater than or equal to 750 kgf / mm 2 Preferably, the Vickers hardness of the reinforced glass ceramic is greater than or equal to 800 kgf / mm 2 The Vickers hardness of the reinforced glass-ceramics is within the above range, indicating that the reinforced glass-ceramics have high hardness and high intrinsic strength, thereby ensuring that they have excellent mechanical properties.
[0173] In some embodiments, the Vickers hardness of the reinforced glass-ceramic may be: 750 kgf / mm 2 、800kgf / mm 2 、805kgf / mm 2 、810kgf / mm 2 、815kgf / mm 2 、820kgf / mm 2 、825kgf / mm 2 、830kgf / mm 2 、835kgf / mm 2 、840kgf / mm 2 ,
[0174] 845kgf / mm 2 、850kgf / mm 2、855kgf / mm 2 、860kgf / mm 2 、865kgf / mm 2 、870kgf / mm 2 、875kgf / mm 2 ,
[0175] 880kgf / mm 2 、885kgf / mm 2 、890kgf / mm 2 、895kgf / mm 2 、900kgf / mm 2 、821kgf / mm 2 、824kgf / mm 2 ,
[0176] 806kgf / mm 2 、812kgf / mm 2 、811kgf / mm 2 、823kgf / mm 2 、804kgf / mm 2 、816kgf / mm 2 、814kgf / mm 2 ,
[0177] 816kgf / mm 2 or 814kgf / mm 2 , or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0178] In some embodiments of the present application, the reinforced glass ceramic is transparent in the visible light wavelength range. Preferably, when the thickness t of the reinforced glass ceramic is 0.40 mm to 1.00 mm, the transmittance of the reinforced glass ceramic for 550 nm wavelength light is ≥ 85%, preferably ≥ 89%.
[0179] Strengthened glass ceramics that meet this transmittance can ensure good optical properties and good transparency, and are suitable for use in electronic device displays that require display effects. The "visible light wavelength range" here refers to light with a wavelength of 360nm-740nm.
[0180] In some embodiments, when the thickness t of the strengthened glass-ceramic is 0.40 mm to 1.00 mm, the transmittance of the strengthened glass-ceramic for light with a wavelength of 550 nm can be: 85.00%, 89.00%, 89.10%, 89.20%, 89.30%, 89.40%, 89.50%, 89.60%, 89.70%, 89.80%, 89.90%, 90.00%, 90.10%, 90. 20%, 90.30%, 90.40%, 90.50%, 91.00%, 92.00%, 89.50%, 89.88%, 89.59%, 89.87%, 89.55%, 89.08%, 89.77%, 89.72% or 89.17%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0181] It should be understood that the reinforced glass ceramic of the present application is made of glass ceramics subjected to chemical strengthening treatment, and the composition at the center of the reinforced glass ceramic is the same or substantially the same as the composition of the glass ceramic. Compared with the glass ceramic before the chemical strengthening treatment (chemical strengthening treatment will perform ion exchange), the composition at the surface of the glass ceramic product after the chemical strengthening treatment may be different from the composition of the glass ceramic before the chemical strengthening treatment. This is because when the chemical strengthening treatment is performed, a type of alkali metal ion (for example, Li ions) at the surface of the glass ceramic in the newly formed glass ceramic is + Or Na + ) will be replaced by alkali metal ions with larger ionic radius (e.g., Na + or K + ) is replaced. However, in an embodiment, the glass composition and phase assembly at or near the depth or thickness center of the glass-ceramic product will still have the composition and phase assembly of the newly formed glass-ceramic. That is, in the present application, the composition (e.g., the composition of the tensile stress layer) and phase assembly at the center of the strengthened glass-ceramic are the same or substantially the same as those of the glass-ceramic that has not been chemically strengthened.
[0182] In the present application, the glass ceramic used to prepare the strengthened glass ceramic can be obtained by heat treating the base glass. The composition of the base glass is the same or substantially the same as that of the glass ceramic in terms of the molar percentage of oxides.
[0183] In some embodiments of the present application, the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass includes: SiO2: 40.00% ~ 50.00%, Al2O3: 20.00% ~ 30.00%, MgO: 3.00% ~ 8.00%, ZnO: 8.00% ~ 12.00%, BaO: 0% ~ 8.00%, CaO: 0% ~ 8.00%, ZrO2: 3.00% ~ 6.00%, Na2O: 2.00% ~ 10.00%, Li2O: 3.00% ~ 12.00%, K2O: 0% ~ 1.00%, Y2O3: 0% ~ 15.00%, La2O3: 0% ~ 15.00%. By adjusting and controlling the content range of each oxide component, it is helpful to ensure that the reinforced glass-ceramics satisfying the desired crystal phase structure is obtained, and it is also helpful to ensure that the reinforced glass-ceramics obtain excellent optical properties and high intrinsic strength.
[0184] In the present application, SiO2 is a glass network former oxide and an indispensable component of the glass network structure. When the content of SiO2 is increased, the stability and mechanical strength of the glass can be increased, but excessive SiO2 will increase the viscosity of the substrate glass, making it more difficult to melt the glass, thereby reducing the formability of the substrate glass. In the present application, the molar percentage of SiO2 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass is 40.00% or more, preferably 40.00% to 50.00%, more preferably 41.00% to 48.00%, and further preferably 42.00% to 47.00%, which is conducive to taking into account the stability, formability and mechanical strength properties of the glass.
[0185] In some embodiments of the present application, the content of SiO2 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, measured by mole percentage of oxide, can be 40.00%, 40.50%, 41.00%, 41.50%, 42.00%, 42.50%, 43.00%, 43.50%, 44.00%, 44.50%, 45.00%, 45.50%, 46.00%, 46.50%, 47.00%, 47.50%, 48.00%, 48.50%, 49.00%, 49.50%, 50.00%, 45.31%, 51.
[0186] 45.76%, 46.29%, 45.13%, 45.85%, 46.76% or 42.52%, or any two of the above
[0187] The specific values are taken as the values within the numerical range formed by the endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0188] In the present application, Al2O3 is one of the components that forms the main crystalline phase (Zn, Mg)Al2O4 after the substrate glass is crystallized, and will directly affect the content of the main crystalline phase (Zn, Mg)Al2O4. As the Al2O3 content increases, the glass phase strength in the glass ceramic is also enhanced, and the mechanical properties of the glass ceramic are enhanced. At the same time, since [AlO4] is larger in volume than [SiO4], it can provide a larger space for ion exchange, which is conducive to promoting chemical strengthening. However, excessive Al2O3 will increase the viscosity of the substrate glass, causing the formability of the substrate glass to decrease. In the present application, the molar percentage of Al2O3 in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is greater than 20%, preferably 20% to 30%, more preferably 22.00% to 29.00%, and further preferably 25.00% to 28.00%.
[0189] In some embodiments of the present application, the content of Al2O3 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, measured by mole percentage of oxide, can be 20.00%, 20.50%, 21.00%, 21.50%, 22.00%, 22.50%, 23.00%, 23.50%, 24.00%, 24.50%, 25.00%, 25.50%, 26.00%, 26.50%, 27.00%, 27.50%, 28.00%, 28.50%, 29.00%, 29.50%, 30.00%, 25.80%, 31.00%, 32.50%, 33.00%, 34.50%, 35.00%, 36.50%, 37.00%, 38.50%, 39.00%, 39.50%, 40.00%, 41.50%, 42.50%, 43.00%, 44.50%, 45.00%, 46.50%, 47.00%, 48.50%, 49.00%, 49.50%, 50.00%, 51.50%, 52.50%, 53.50%, 54.00%, 55.50%, 56.00%, 57.50%, 58.50%, 59.00%, 60.50%, 61.00%, 61.50%, 62.50%, 63.50%, 64.00%, 65.50%, 66.00%, 67.50%, 68.00%, 69
[0190] 27.03%, 26.36%, 25.70%, 26.10%, 26.62% or 27.36%, or a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0191] In the present application, ZnO provides the zinc necessary for the substrate glass to form the main crystalline phase (Zn, Mg) Al2O4 after crystallization. ZnO can reduce the thermal expansion coefficient of the glass and improve the chemical stability, thermal stability and refractive index of the glass. MgO provides the magnesium necessary for the substrate glass to crystallize and form the main crystalline phase (Zn, Mg) Al2O4. MgO can slow down the hardening speed of the glass and improve the forming properties of the glass; MgO can also reduce the crystallization tendency and crystallization speed, increase the high temperature viscosity of the glass, and improve the chemical stability and mechanical strength of the glass. However, the addition of excessive MgO and ZnO often leads to excessively large spinel grains, making it difficult to obtain glass ceramics with high transparency. In the present application, the composition at the center of the reinforced glass-ceramic or the composition of the glass-ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass is as follows: the molar percentage of ZnO is 8.00% to 12.00%, preferably 8.50% to 11.50%, and more preferably 9.00% to 11.00%; the molar percentage of MgO is 3.00% to 8.00%, preferably 4.00% to 7.00%, and more preferably 5.00% to 6.00%.
[0192] In some embodiments of the present application, the content of ZnO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 9.71%, 9.80%, 10.91%, 9.67%, 9.82%, 9.92%, 10.02% or 9.96%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0193] In some embodiments of the present application, the content of MgO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 5.47%, 5.52%, 5.59%, 5.45%, 5.53%, 5.64% or 5.80% in terms of molar percentage of oxide, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0194] In the present application, BaO is an optional component. An appropriate amount of BaO can improve the melting effect of glass, increase the density of glass, improve Young's modulus, and inhibit the growth of grains to a certain extent, thereby improving the optical properties of glass ceramics. However, the presence of too much BaO has a strong inhibitory effect on the exchange process of Na ions and K ions. In the present application, the molar percentage of BaO in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 0% to 8.00%, preferably 0% to 5.00%, and more preferably 0% to 4.00%.
[0195] In some embodiments of the present application, the content of BaO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 1.16%, 1.17%, 0% or 3.47%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0196] In the present application, CaO is an optional component. An appropriate amount of CaO can improve the chemical stability and mechanical properties of the glass, reduce the melting temperature and high-temperature viscosity of the glass, and promote the melting and clarification of the glass liquid. However, when the CaO content is too high, it will increase the crystallization tendency of the glass, reduce the thermal stability of the glass, and increase the annealing temperature. In the present application, the molar percentage of CaO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass is 0% to 8.00%, preferably 0% to 3.00%, and more preferably 0% to 1.50%.
[0197] In some embodiments of the present application, in terms of molar percentage of oxide, the content of CaO in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00% or 0.99%, or can be a value within a numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0198] In the present application, ZrO2 is an effective nucleating agent. During the heat treatment of glass, ZrO2 is first precipitated in the form of crystals, and the ZrO2 crystals become crystal nuclei for the subsequent crystal growth. Within a certain glass composition range, the content of ZrO2 will affect the formation of glass, the crystal shape, crystal type and crystal size of glass ceramics after glass heat treatment, etc. By regulating the glass composition, ZrO2 can be preferentially precipitated at the same temperature, and then the main crystal phase spinel crystal growth can be achieved. When the ZrO2 content is too low, it will affect the precipitation of the main crystal phase zinc-magnesium spinel solid solution crystal phase; when the ZrO2 content is too high, it will cause the melting difficulty of the substrate glass to become greater, resulting in the production of white unmelted materials in the substrate glass. In the present application, the molar percentage of ZrO2 in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 3.00% to 6.00%, preferably 3.00% to 5.00%, and more preferably 3.10% to 4.00%.
[0199] In some embodiments of the present application, the content of ZrO2 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 3.00%, 3.20%, 3.50%, 3.70%, 4.00%, 4.20%, 4.50%, 4.70%, 5.00%, 5.20%, 5.50%, 5.70%, 6.00%, 3.39%, 3.42%, 3.46%, 3.38%, 3.43% or 3.48%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramic or strengthened glass-ceramic with the desired performance of the present application can be obtained.
[0200] In the present application, the increase of Na2O content helps to obtain higher surface compressive stress, and can also reduce the melting temperature and the temperature of crystal precipitation. However, excessive addition of Na2O will cause the glass to ceramicize during annealing, or cause the precipitation of other impurities that affect the transmittance of glass ceramics during heat treatment. Too low Na2O content will lead to increased heat treatment temperature, direct phase separation or precipitation of impurities during heat treatment, and obtain opaque or poorly transparent glass ceramics. In the present application, the molar percentage of Na2O in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 2.00% to 10.00%, preferably 2.50% to 8.00%, and more preferably 3.00% to 6.00%.
[0201] In some embodiments of the present application, the content of Na2O in the composition at the center of the strengthened glass-ceramic, the composition of the glass-ceramic used to prepare the strengthened glass-ceramic, or the composition of the substrate glass, measured by molar percentage of oxide, can be 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 3.39%, 3.43%, 3.47%, 3.38%, 5.39% or 3.55%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic having the desired properties of the present application can be obtained.
[0202] In the present application, Li2O helps to obtain a higher depth of the compressive stress layer and improve the Young's modulus; at the same time, it can reduce the melting temperature and the temperature of crystal precipitation, but its excessive addition will cause the glass to ceramicize during the annealing process, or cause the precipitation of other impurities that affect the transmittance of the glass ceramic during the heat treatment, or cause excessive crystal growth during the heat treatment, so that the transmittance of the obtained glass ceramic decreases. If the amount of Li2O added is too low, the heat treatment temperature will increase and the deep stress will decrease. In the present application, the molar percentage of Li2O in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass is 3.00% to 12.00%, preferably 3.20% to 10.00%, and more preferably 3.50% to 6.00%.
[0203] In some embodiments of the present application, the content of Li2O in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, measured by molar percentage of oxide, can be 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 5.77%, 3.87%, 3.92%, 5.75%, 3.88%, 4.91%, 3.96% or 3.86%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass-ceramic or strengthened glass-ceramic with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic having the desired properties of the present application can be obtained.
[0204] In the present application, K2O is an optional component, and its molar percentage can be 0% to 1.00%. In some embodiments, preferably, the composition at the center of the reinforced glass-ceramic or the composition of the glass ceramic used to prepare the reinforced glass-ceramic or the composition of the substrate glass does not contain K2O.
[0205] In the present application, rare earth oxides Y2O3 and / or La2O3 are optional components, and the addition of an appropriate amount can improve the strength of glass ceramics. Y2O3 is an optional component that improves the hardness and chemical stability of glass ceramics and inhibits glass forming and crystallization. An appropriate amount of Y2O3 can improve the density of the glass phase, thereby improving the overall strength of glass ceramics. Y2O3 can form a eutectic with ZrO2, and when melted in a furnace, it reduces the problem of glass inhomogeneity caused by ZrO2 precipitation. However, excessive Y2O3 content affects the precipitation of spinel crystals of the main crystal phase in glass ceramics, resulting in a decrease in the optical properties of glass ceramics, while reducing the chemical strengthening properties of glass ceramics. An appropriate amount of La2O3 can improve the density of glass ceramics, improve dielectric constant, mechanical strength, chemical stability, etc., and increase hardness and softening temperature. In the present application, the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass is as follows: the molar percentage of Y2O3 is 0% to 15.00%, preferably 0% to 5.00%, more preferably 0% to 1.00%; the molar percentage of La2O3 is 0% to 15.00%, preferably 0% to 5.00%, more preferably 0% to 1.00%.
[0206] In some embodiments of the present application, the content of Y2O3 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.0 ... %, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 12.50%, 13.00%, 13.50%, 14.00%, 14.50%, 15.00% or 0.19%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0207] In some embodiments of the present application, the content of La2O3 in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass can be 0%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.0 ... 0%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 12.50%, 13.00%, 13.50%, 14.00%, 14.50%, 15.00% or 0.19%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0208] In the present application, on the basis of adjusting and controlling the content range of each oxide component, by adjusting and controlling the ratio between the oxide components, adding an appropriate amount of Y2O3 and / or La2O3 is beneficial to improving the strength, hardness, stability and deformation resistance of the reinforced glass-ceramics.
[0209] In some embodiments of the present application, in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, the molar percentage of Y2O3 [Y2O3] and the molar percentage of La2O3 [La2O3] satisfy the following relationship: 0%<[Y2O3]+[La2O3]≤15.00%; preferably, 0%<[Y2O3]+[La2O3]≤5.00%, and more preferably, 0%<[Y2O3]+[La2O3]≤1.00%.
[0210] In some embodiments, in the composition at the center of the strengthened glass-ceramic or the composition of the glass-ceramic used to prepare the strengthened glass-ceramic or the composition of the substrate glass, the sum of the molar percentage of Y2O3 [Y2O3] and the molar percentage of La2O3 [La2O3], [Y2O3] + [La2O3] can be 0.05%, 0.10%, 0.20%, 0.30%, 0.40%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00% %, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 12.50%, 13.00%, 13.50%, 14.00%, 14.50%, 15.00% or 0.38%, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0211] In the present application, in order to obtain the desired strengthened glass ceramics with excellent performance, in addition to Y2O3 and La2O3, in terms of oxides, metal oxides of cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium or scandium, or mixtures of the aforementioned metal oxides, can be added to the composition of the glass ceramic or the composition of the substrate glass used to prepare the strengthened glass ceramics, as long as the glass ceramics or strengthened glass ceramics with the desired performance of the present application can be obtained. If the aforementioned metal oxides are added to the composition of the glass ceramic or the composition of the substrate glass used to prepare the strengthened glass ceramics, the composition at the center of the obtained strengthened glass ceramics should also contain these metal oxides.
[0212] In some embodiments of the present application, since the addition of P2O5 is likely to affect the optical properties of the glass ceramic or the strengthened glass ceramic, the addition of B2O3 can improve the melting effect of the substrate glass, but it is likely to affect the toughness and other properties of the strengthened glass ceramic. The addition of TiO2 is likely to cause the glass ceramic or the strengthened glass ceramic to present an undesirable color. Therefore, it is preferred that the glass ceramic or the strengthened glass ceramic of the present application does not contain P2O5, B2O3 or TiO2. In some embodiments, in terms of molar percentage of oxides, in the composition at the center of the strengthened glass ceramic or the composition of the glass ceramic used to prepare the strengthened glass ceramic or the composition of the substrate glass: does not contain P2O5, and / or, does not contain B2O3, and / or, does not contain TiO2.
[0213] In some embodiments of the present application, the crystallinity of the glass ceramic or reinforced glass ceramic is 30% to 55%, preferably 40% to 55%. In some embodiments, the crystallinity of the glass ceramic or reinforced glass ceramic can be 30%, 35%, 40%, 45%, 55%, 47%, 48%, 41%, 50%, 51% or 46%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0214] In the present application, "main crystalline phase zinc aluminum spinel-magnesium aluminum spinel solid solution" or "using zinc aluminum spinel-magnesium aluminum spinel solid solution as the main crystalline phase of glass ceramics" or other similar expressions means that the zinc aluminum spinel-magnesium aluminum spinel solid solution accounts for more than 50% by mass of all crystalline phases of the glass ceramics or reinforced glass ceramics according to the embodiments of the present application. In some embodiments, the mass of the zinc aluminum spinel-magnesium aluminum spinel solid solution accounts for more than 50% of all crystalline phases of the glass ceramics or the reinforced glass ceramics used to prepare the reinforced glass ceramics, and preferably, the mass of the zinc aluminum spinel-magnesium aluminum spinel solid solution accounts for more than 70% of all crystalline phases of the glass ceramics or the reinforced glass ceramics used to prepare the reinforced glass ceramics. Exemplarily, in the glass ceramic used to prepare the strengthened glass ceramic or all the crystalline phases of the strengthened glass ceramic, the mass proportion (or also called, weight proportion) of the zinc aluminum spinel-magnesium aluminum spinel solid solution crystalline phase can be 50%, 60%, 70%, 79%, 80%, 81%, 82%, 83%, 84%, 85% or 86%, or can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or strengthened glass ceramic with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or strengthened glass ceramic with the required performance of the present application can be obtained.
[0215] In some embodiments of the present application, in the glass ceramic or reinforced glass ceramic, the average crystal size does not exceed 20nm, preferably 1nm to 15nm, and more preferably 3nm to 8nm. In some embodiments, in the glass ceramic or reinforced glass ceramic, the average crystal size can be 4nm, 5.6nm, 5.7nm, 6.9nm, 6.4nm, 7.3nm, 5.6nm, 6.6nm, 6.1nm or 5.5nm, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass ceramic or reinforced glass ceramic with the desired performance of the present application can be obtained.
[0216] By making the glass ceramic or reinforced glass ceramic meet the desired crystallinity and appropriate average grain size, the glass ceramic or reinforced glass ceramic can maintain excellent optical properties while meeting excellent mechanical strength properties and high intrinsic strength.
[0217] In some embodiments of the present application, the reinforced glass ceramic, after the sand and stone scratch test, has a haze growth factor of less than 3.00, preferably a haze growth factor of less than 2.50, and more preferably a haze growth factor of less than 2.10, compared with the haze of the reinforced glass ceramic before the sand and stone scratch test;
[0218] Among them, the sand and gravel scratch test refers to placing the reinforced glass ceramics and 1kg of silica sand in an oscillating abraser for scratch testing. The oscillation frequency of the oscillating abraser is 150 rpm, and the time of the sand and gravel scratch test is 10 minutes. In the present application, the anti-scratch performance of the embodiments and comparative examples is reflected / characterized by the haze growth multiple after the scratch test. The larger the haze growth multiple, the worse the scratch resistance of the product, and the more serious the damage it suffers in the scratch test. The smaller the haze growth multiple, the better the scratch resistance of the product, and the less damage it suffers in the scratch test. The reason why the haze growth multiple can reflect the scratch resistance is mainly because the scratches on the surface of the glass product will directly affect the haze of the glass product, and affect the optical properties and display effects of the glass product. Fig. 9 As shown, Figure a is a physical picture of the reinforced glass ceramic of Example 4 after the sand and stone scratch test, and its haze growth factor is 0.19, and Figure b is a physical picture of the reinforced glass ceramic of Example 2 after the sand and stone scratch test, and its haze growth factor is 9.72.
[0219] In some embodiments, the haze of the reinforced glass-ceramic after the sand and stone scratch test can be increased by less than 1.80 times, less than 1.60 times, less than 1.50 times, less than 1.20 times, or less than 1.00 times compared to the haze of the reinforced glass-ceramic before the sand and stone scratch test. In some embodiments, the haze increase factor can be 0.10 times, 0.20 times, 0.30 times, 0.40 times, 0.5 times 0, 0.6 times 0, 0.70 times, 0.80 times, 0.90 times, 1.00 times, 1.10 times, 1.20 times, 1.30 times, 1.40 times, 1.50 times, 1.60 times, 1.70 times, 1.80 times, 1.90 times, 2.00 times, 2.10 times, 2.20 times, 2.30 times, 2.40 times, 2.5 0 times, 2.60 times, 2.70 times, 2.80 times, 2.90 times, 3.00 times, 0.22 times, 0.69 times, 1.15 times, 0.19 times, 1.46 times, 1.81 times, 1.56 times, 1.59 times, 2.03 times, 1.02 times, 0.76 times, 1.02 times or 0.88 times, or it can be a value within the numerical range consisting of any two of the above specific values as endpoints, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the reinforced glass-ceramic with the desired performance of the present application can be obtained.
[0220] After introducing the composition, crystal phase and stress structure of strengthened glass-ceramics, the preparation method of strengthened glass-ceramics is introduced in detail below.
[0221] In the present application, the preparation process of strengthened glass ceramics mainly includes: the preparation process of glass ceramics and the chemical strengthening treatment process, and the preparation process of glass ceramics mainly includes: the preparation process of substrate glass and the heat treatment process of substrate glass.
[0222] In the present application, the substrate glass can be prepared by a molding method in the prior art, and the present application has no limitation on this. For example, the molding method of the substrate glass can include but is not limited to float, overflow, rolling or casting processes. For example, the substrate glass can be obtained by uniformly mixing the components according to the formula, melting and molding, cooling and annealing.
[0223] Exemplarily, each raw material (conventional industrial raw material) is configured according to the formula ratio, a clarifier is added, and then mixed for a period of time to obtain a uniform raw material mixture. The raw material mixture is placed in a platinum crucible, heated to 1450°C to 1800°C, preferably the melting temperature is 1550°C to 1680°C, and preferably kept warm for 3 to 15 hours under this temperature condition, and then poured into a molding mold for cooling and molding, preferably cooled to 800°C to 1000°C, and then placed in an annealing furnace for annealing treatment, preferably the annealing temperature is 500°C to 700°C, and the annealing time is preferably 5 to 48 hours; then cooled to room temperature with the furnace, the substrate glass can be obtained. Those skilled in the art can select the type and amount of clarifier according to needs, and they do not need to pay creative labor. Further, the clarifier may include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the amount of clarifier added may be 0wt%-1wt% of the total amount of each raw material.
[0224] In some embodiments of the present application, the heat treatment process of the substrate glass may include a nucleation treatment and / or a crystallization treatment, preferably a nucleation treatment and a crystallization treatment. In some embodiments, the crystallization treatment includes a one-step crystallization treatment or a two-step crystallization treatment.
[0225] In some embodiments of the present application, in order to obtain the desired physical and chemical properties of the glass ceramic, when the substrate glass is heat treated, a one-step heat treatment may be performed, or two-step or multi-step heat treatment may be performed. If a one-step heat treatment is performed, it means that a nucleation treatment (i.e., nucleation treatment) is not performed separately, and a one-step heating is directly performed, and nucleation and target crystal growth are performed at the temperature reached in the one-step heating process, which can be understood as a direct crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, first a nucleation treatment, i.e., nucleation treatment, is performed, and then a target crystal growth treatment, i.e., crystallization treatment, is performed.
[0226] In order to make the glass ceramics precipitate the desired crystalline phase and obtain the desired physical and chemical properties, further, the temperature of the nucleation treatment can be 600-850°C, and the time of the nucleation treatment can be 0-72h, preferably 0-10h; the temperature of the crystallization treatment can be 700-1000°C, and the time of the crystallization treatment can be 0.10-24h, preferably 0.1-6h. When performing heat treatment, it is preferred to control the heating rate to 5-15°C / min, and more preferably the heating rate is 10°C / min. Among them, the temperature of the nucleation treatment refers to the temperature at which the crystal nucleus can be formed. The temperature of the crystallization treatment refers to the temperature at which the target crystal is suitable for controllable growth.
[0227] After heat treatment, technicians in this field can also perform other conventional steps to obtain glass-ceramic samples / samples that meet the required specifications or requirements, such as shaping, cutting (such as cutting using a multi-wire cutting machine), CNC machining (computer numerical control, i.e., CNC machine tools), thinning or polishing.
[0228] In some embodiments of the present application, by subjecting the aforementioned glass-ceramics to a specific chemical strengthening treatment, a strengthened glass-ceramic satisfying the desired performance can be prepared.
[0229] In the present application, the chemical strengthening treatment, i.e., the ion exchange method, is performed by immersing the glass ceramic in a molten salt bath to exchange the alkali metal ions with smaller ion radius in the glass ceramic with the alkali metal ions with larger ion radius in the molten salt bath, thereby forming a compressive stress layer on the surface of the glass ceramic to obtain strengthened glass ceramics with better mechanical properties.
[0230] In some embodiments of the present application, the chemical strengthening treatment may adopt a single-step strengthening method or a multi-step strengthening method. The molten salt bath for chemical strengthening treatment is a molten salt bath containing sodium salt and / or potassium salt. Preferably, the chemical strengthening of the present application adopts a two-step strengthening method, and the molten salt bath used in each strengthening process is a pure salt bath containing sodium salt or potassium salt. Preferably, the temperature of the molten salt bath is 380°C to 600°C, and more preferably 400°C to 500°C. In some embodiments of the present application, a certain amount (e.g., 0wt%-0.5wt%) of lithium salt may be added to the salt bath. In some embodiments of the present application, the preferred time for chemical strengthening treatment is 0.1h to 48h, preferably 0.1h to 24h. Among them, the sodium salt can be selected from at least one of sodium nitrate, sodium sulfate, and sodium carbonate, preferably sodium nitrate; the potassium salt can be selected from at least one of potassium nitrate, potassium sulfate, and potassium carbonate, preferably potassium nitrate; the lithium salt can be selected from at least one of lithium nitrate, lithium sulfate, and lithium carbonate, preferably lithium nitrate.
[0231] The glass ceramics or strengthened glass ceramics with excellent performance (especially excellent scratch resistance) provided in the present application can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), vehicle-mounted central control, electronic whiteboard glass, smart home, smart wear (such as smart bracelets, smart watches, smart glasses), and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass devices of glass ceramics or strengthened glass ceramics. For example, it can be used for display screens, cover glass, touch screens, glass inner screens or inner frames of electronic devices; for example, it can be used for windshields of vehicles, aircraft or aircraft, such as front windshields or side windshields. For example, it can be used for worktops, other surfaces, appliance doors, floor tiles, wall panels or storage containers. Other surfaces can include but are not limited to exterior wall surfaces, stair tread surfaces, column veneers or counter surfaces, and storage containers can include but are not limited to cups, plates, medicine bottles or beverage bottles.
[0232] For example, the glass ceramics or reinforced glass ceramics with excellent performance provided in the present application can be used to manufacture glass devices. The glass devices referred to here can be regular or irregular, and those skilled in the art can manufacture them according to needs.
[0233] For example, the glass ceramic or reinforced glass ceramic with excellent performance (especially excellent scratch resistance) provided by the present application can be used to manufacture cover glass, and the cover glass can be a display cover, back cover or camera protection cover of an electronic device. For example, the glass ceramic or reinforced glass ceramic with excellent performance (especially excellent scratch resistance) provided by the present application can be used in electronic devices. Figure 2 , Figure 3 , Figure 4 and Figure 8 In some embodiments of the present application, an electronic device is provided, which may be a mobile phone (such as Figure 2 ), tablet computers, smart wearable devices (such as Figure 8) and other electronic products, the electronic device includes a shell 1 assembled on the outside of the electronic device, the shell 1 includes a display screen cover 11 assembled on the front side and a back cover 12 assembled on the back side, the display screen cover 11 is covered on the display module 4, wherein the display screen cover 11 and / or the back cover 12 are made of the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the display screen cover 11 and the back cover 12 may be made of the aforementioned glass ceramics or reinforced glass ceramics in their entirety, or only partially of the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the display screen may be a touch screen, and the display screen cover 11 may be a protective cover provided on the touch screen. In the present application, the back cover 12 may cover only the back side (and the side away from the display screen) of the electronic device, or may cover both the back side and the side frame of the electronic device. Optionally, the back cover 12 may cover all the side frames around the electronic device, or may cover part of the side frames.
[0234] In some implementation modes of the present application, Figure 3 As shown, the electronic device may further include a camera assembly 2 located inside the housing 1, and the housing 1 may include a camera protection cover 13, the camera protection cover 13 is covered on the camera assembly 2 for protecting the camera assembly 2, and the camera protection cover 13 adopts the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the camera protection cover 13 may be partially made of the aforementioned glass ceramics or reinforced glass ceramics, or may be entirely made of the aforementioned glass ceramics or reinforced glass ceramics. In the present application, the setting position of the camera protection cover 13 is determined according to the setting position of the camera assembly 2, and may be located on the front side of the electronic device, or may be located on the back side of the electronic device. In some embodiments of the present application, the camera protection cover 13 may be a separate structure from the display screen cover 11 or the back cover 12. In other embodiments of the present application, the camera protection cover 13 may also be an integrated structure with the display screen cover 11 or the back cover 12.
[0235] In some embodiments of the present application, Figure 4 As shown, the electronic device may further include a middle frame 3 located between the display module 4 and the housing 1 , and the middle frame 3 may include the aforementioned glass ceramic or reinforced glass ceramic.
[0236] In the embodiments of the present application, the display cover, back cover, camera protection cover, and middle frame in the electronic device may be made of the aforementioned glass ceramics or reinforced glass ceramics for any one of the four, or any two of them may be made of the aforementioned glass ceramics or reinforced glass ceramics, or all three may be made of the aforementioned glass ceramics or reinforced glass ceramics, or all four may be made of the aforementioned glass ceramics or reinforced glass ceramics.
[0237] In some embodiments of the present application, the display screen cover, back cover, camera protection cover or middle frame in the electronic device may be 2D, 2.5D, 3D or special-shaped. In some embodiments of the present application, the display screen cover, back cover, camera protection cover or middle frame in the electronic device may be of equal thickness or unequal thickness.
[0238] The technical solution of the present application is further described in detail below in conjunction with the embodiments. The embodiments of the present application described in detail below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0239] Example 1
[0240] A reinforced glass ceramic, the preparation process of which is as follows:
[0241] (1) Preparation of substrate glass:
[0242] The raw materials (conventional industrial raw materials) were prepared according to the proportions of the components in Table 1. The total mass of the prepared raw materials was 1000 g. 5 g of clarifier sodium chloride (NaCl) was added to the prepared raw materials, and then mixed with a V-type mixer for 30 minutes to obtain a uniform raw material mixture.
[0243] The raw material mixture is transferred to a platinum crucible, and then melted in a platinum crucible at 1650°C for 5 hours, and then poured into a molding mold preheated at 300°C for molding and cooling, cooled to 900°C, and then placed in a 600°C annealing furnace for annealing for 24 hours, and then cooled to room temperature with the furnace to obtain the base material glass brick.
[0244] (2) Preparation of glass ceramics:
[0245] According to the heat treatment process in Table 2, the substrate glass brick is placed in an annealing furnace, and the temperature is raised from room temperature to 750°C at a heating rate of 10°C / min for nucleation treatment. After heat treatment at this temperature for 240 minutes, the temperature is raised to 755°C at a heating rate of 10°C / min for crystallization treatment. The temperature is kept at this temperature for 150 minutes, and then the temperature is lowered to room temperature at a cooling rate of 1°C / min to obtain a glass ceramic sample brick. In terms of the molar percentage of oxides, the composition of the obtained glass ceramic is the same as that of the substrate glass, as shown in Table 1.
[0246] The obtained glass ceramic sample bricks are subjected to the cold working treatment of cutting, CNC processing (the CNC instrument model used in this application is: RCG500S), and polishing in sequence, and glass ceramic samples / samples that meet the required specifications and requirements can be obtained. In Examples 1 to 15 and Comparative Examples 1 to 20 of the present application, the glass ceramic sample bricks are subjected to the aforementioned cold working treatment to be made into glass ceramic samples / samples with a thickness of 0.70mm, 0.40mm, 0.90mm or 1.00mm, specifically, glass ceramic polished sheet samples of 50mm×50mm×0.70mm, 50mm×50mm×0.40mm, 50mm×50mm×0.90mm, 50mm×50mm×1.00mm, φ46mm×0.70mm, φ46mm×0.40mm, φ46mm×0.90mm or φ46mm×1.00mm are made. 50mm×50mm×0.70mm is a square glass piece with a length of 50mm, a width of 50mm and a thickness of 0.70mm; φ46mm×0.70mm is a round glass piece with a diameter of 46mm and a thickness of 0.70mm. The meanings of other sizes are similar.
[0247] The glass ceramic samples / samples obtained in Example 1 were tested as follows:
[0248] The crystal phase composition, crystallinity, average crystal size, transmittance (under 550 nm wavelength light) and density of the glass-ceramic samples / specimens were tested respectively, and the results are shown in Table 2.
[0249] (3) Preparation of strengthened glass ceramics: According to the chemical strengthening process in Table 3, the obtained glass ceramic sample / sample is placed in the strengthening furnace cavity for preheating for 5 minutes, and then quickly placed in a molten salt bath at 455°C for the first step of strengthening treatment. The composition of the molten salt bath used for the first step of strengthening treatment is 100wt% NaNO3, and the strengthening treatment time is 3.5h. After the strengthening is completed, it is cooled, cleaned, and dried to ensure that there is no sodium salt. The glass ceramic sample / sample is placed in a molten salt bath at 420°C for the second step of strengthening treatment. The composition of the molten salt bath used for the second step of strengthening treatment is 100wt% KNO3, and the strengthening treatment time is 3.5h. After the second step of strengthening treatment, take out the glass ceramic sample / sample and place it on the strengthening furnace body to slowly cool to room temperature, then wash off the salt wrapped on the surface of the glass ceramic with clean water, and after the glass ceramic sample / sample is dried, the strengthened glass ceramic can be obtained.
[0250] The results of testing the reinforced glass ceramics obtained in Example 1 are as follows:
[0251] Ⅰ. The strengthened glass-ceramics were measured for CS_20, CS_30, CS_50 and DOL_0 using a SLP-2000 stress meter (the light source wavelength used was 518 nm, SOC=25.5 (nm / cm) / MPa, the refractive index was set to 1.60, and the exposure time was 300 μsec). The results are shown in Table 3.
[0252] Ⅱ. The strengthened glass ceramics were subjected to micro-area composition analysis using Shimadzu electron probe EPMA-1720HT, using the characteristic X-rays generated by the electron beam acting on the sample / specimen, and DOL_K was measured. The results are shown in Table 3.
[0253] Based on the measured CS_20, CS_30, CS_50, DOL_0 and DOL_K, the value of formula X was calculated and the results are shown in Table 3.
[0254] III. The Vickers hardness of the reinforced glass-ceramics was tested, and the haze growth multiple of the reinforced glass-ceramics was calculated after the scratch test. The results are shown in Table 3.
[0255] Example 2 to Example 15
[0256] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, different process parameters and corresponding test results of each example are shown in Tables 1 to 3, respectively.
[0257] Among them, the XRD spectrum comparison diagram of the glass ceramic of Example 1 and the reinforced glass ceramic is as follows: Figure 5 As shown in the figure, ① the main crystal phase of the glass ceramic and the strengthened glass ceramic is zinc aluminum spinel-magnesium aluminum spinel solid solution (Zn, Mg)Al2O4, and the secondary crystal phase is ZrO2; ② the XRD spectra of the glass ceramic and the strengthened glass ceramic are basically overlapped, and the crystal phase structure is basically unchanged before and after chemical strengthening.
[0258] The transmittance curve comparison of the glass ceramic of Example 1 and the reinforced glass ceramic is shown in FIG. Figure 6 As shown in the figure, it can be seen that the glass ceramics and the strengthened glass ceramics prepared therefrom are both transparent in the visible light range, both have high transmittance, and the transmittance remains basically unchanged before and after chemical strengthening.
[0259] Comparative Examples 1 to 3, Comparative Examples 5 to 20
[0260] The methods are respectively carried out with reference to Example 1, except that the raw material compositions, different process parameters and corresponding test results of each comparative example are shown in Tables 1 to 3, respectively.
[0261] Comparative Example 4 is a coated glass product (AF-coated glass product) with model number SP194 sold by Shenzhen Green Link Technology Co., Ltd., which was purchased directly.
[0262] Among them, the micrographs of the scratch points of the reinforced glass ceramics provided in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 after the sand and stone scratch test are as follows: Figure 7 As shown in the figure, the black points in the figure are scratch points, or also called damage points, such as the points circled in the picture. Among them, a is a micrograph of the scratch points of Example 1, b is a micrograph of the scratch points of Example 2, c is a micrograph of the scratch points of Comparative Example 1, and d is a micrograph of the scratch points of Comparative Example 2. It can be seen from the figure that the scratch resistance of the strengthened glass ceramic provided in the embodiment of the present application is significantly better than that of the comparative example.
[0263] The actual comparison diagram of the strengthened glass ceramics provided in Example 4 and Comparative Example 2 after the sand and stone scratch test is as follows: Fig. 9 As shown. Fig. 9 It can be seen that the scratch resistance of the strengthened glass ceramics provided in the embodiment of the present application is significantly better than that of the comparative example. After the scratch test, the optical properties of the strengthened glass ceramics of the embodiment are less affected, while the optical properties of the strengthened glass ceramics of the comparative example are more affected.
[0264]
[0265]
[0266]
[0267]
[0268]
[0269]
[0270] It can be obtained from the embodiments and comparative examples of Tables 1 to 3 above that each embodiment of the present application can give glass ceramics high intrinsic strength (or also known as inherent strength) by making the reinforced glass ceramics meet a specific crystal phase structure and using zinc aluminum spinel-magnesium aluminum spinel solid solution as the main crystal phase of glass ceramics. At the same time, the present application makes the surface of the reinforced glass ceramics with high intrinsic strength have a specific stress distribution structure by making the stress at different depth positions on the surface of the reinforced glass ceramics, the K ion diffusion depth (or also known as the K ion exchange (layer) depth) and the compression stress layer depth meet the requirements of formula X, thereby making the reinforced glass ceramics have excellent scratch resistance. In this application, the anti-scratch performance of the embodiment and comparative example products is embodied / characterized by the haze growth multiple after the scratch test. The larger the haze growth multiple, the worse the scratch resistance of the product, and the more serious the damage it suffers in the scratch test. The smaller the haze growth multiple, the better the scratch resistance of the product, and the less damage it suffers in the scratch test. The reason why the haze growth multiple can reflect the anti-scratch performance is mainly because scratches on the surface of glass products will directly affect the haze of glass products, affecting the optical properties and display effects of glass products.
[0271] In the schemes of Comparative Examples 1 to 20, the crystal structure or surface stress distribution of the strengthened glass ceramics or strengthened glass or coated glass does not meet the specific requirements of the present application, and the scratch resistance of the finally obtained strengthened glass ceramics is obviously inferior to the embodiments that meet the requirements of the scheme of the present application.
[0272] The data of each embodiment and comparative example are specifically analyzed below:
[0273] In Example 1, after chemical strengthening treatment, the Vickers hardness of the obtained strengthened glass ceramic is 850 kgf / mm 2 , which indicates that the chemical strengthening treatment forms a compressive stress structure on the surface of the glass ceramic, which can improve the mechanical properties of the glass ceramic. The reinforced glass ceramic prepared in Example 1 was scratched with sand and gravel. After the scratch test, the haze increase factor of the reinforced glass ceramic was only 0.22, which indicates that the reinforced glass ceramic of Example 1 has excellent scratch resistance, and the friction between the sand and gravel and the reinforced glass ceramic surface hardly causes damage. The surface micrograph of the reinforced glass ceramic of Example 1 after the scratch test is shown in the figure. Figure 7 As shown in a.
[0274] In Example 2, the Vickers hardness of the obtained reinforced glass ceramic is 810 kgf / mm 2 The scratch test was carried out with sand and stone. The test conditions were the same as those in Example 1. After the scratch test, the haze of the reinforced glass ceramic increased by a multiple of 0.69. The friction between the sand and stone and the surface of the reinforced glass ceramic almost did not cause any damage. The surface micrograph of the reinforced glass ceramic of Example 2 after the scratch test is shown in FIG. Figure 7 As shown in b.
[0275] Since the other embodiments are basically similar to Embodiment 1 and Embodiment 2, they are not described in detail here.
[0276] In Comparative Example 1, the glass ceramics prepared have petalite and lithium disilicate as the main crystal phases. After chemical strengthening treatment, the Vickers hardness of the obtained strengthened glass ceramics is 712 kgf / mm 2 , the hardness of the reinforced glass ceramic is much lower than that of the glass ceramic with spinel as the main crystal phase. The reinforced glass ceramic prepared in Comparative Example 1 was subjected to a scratch test with sand and gravel. The test conditions were the same as those in Example 1. After the scratch test, the haze of the reinforced glass ceramic increased by a multiple of 6.5, which shows that the scratch resistance of the reinforced glass ceramic in Comparative Example 1 is far inferior to that of the solution in the embodiment of the present application. After the sand and gravel scratch test, the surface of the reinforced glass ceramic in Comparative Example 1 was severely damaged, resulting in a significant increase in its haze. The surface micrograph of the reinforced glass ceramic in Comparative Example 1 after the scratch test is shown in the figure below. Figure 7 As shown in c.
[0277] Comparative Example 2 has the same crystal phase composition as Comparative Example 1. In Comparative Example 2, after chemical strengthening treatment, the surface stress level of the strengthened glass-ceramic obtained in Comparative Example 2 is higher than that of Comparative Example 1, and the Vickers hardness of the strengthened glass-ceramic is 730 kgf / mm 2 . The reinforced glass ceramics prepared in Comparative Example 2 were subjected to a scratch test with sand and gravel. The test conditions were the same as those in Example 1. After the scratch test, the haze of the reinforced glass ceramics increased by a multiple of 9.72. Like Comparative Example 1, the scratch resistance of the reinforced glass ceramics in Comparative Example 2 is far inferior to that of the solution in the embodiment of the present application. After the sand and gravel scratch test, the surface of the reinforced glass ceramics in Comparative Example 2 was also severely damaged, resulting in a significant increase in its haze. The surface micrograph of the reinforced glass ceramics in Comparative Example 2 after the scratch test is shown in FIG. Figure 7 As shown in middle d.
[0278] In Comparative Example 3, a tempered glass without crystals and with relatively excellent performance is provided. After chemical strengthening, the Vickers hardness of the obtained tempered glass is 685 kgf / mm 2 The hardness of the tempered glass is obviously much lower than that of the glass ceramic with spinel as the main crystal phase. The tempered glass prepared in Comparative Example 3 was scratched with sand and stone, and the test conditions were the same as those in Example 1. After the scratch test, the haze increase factor of the tempered glass after strengthening was 17.67. This shows that the scratch resistance of the tempered glass in Comparative Example 3 is far inferior to that of the embodiment of the present application.
[0279] In Comparative Example 4, a coated glass product of Shenzhen Green Link Technology Co., Ltd. is provided, the product model is SP194, specifically an AF coated glass product, and its Vickers hardness is 598kgf / mm 2The coated glass provided in Comparative Example 4 was subjected to a scratch test with sand and gravel, and the test conditions were the same as those in Example 1. After the scratch test, the AF film on the surface of the coated glass was worn away by the sand and gravel, and the haze increase factor of the coated glass was 8.9. Although it was more scratch-resistant than the uncoated tempered glass of Comparative Example 3, its scratch resistance was far inferior to the tempered glass ceramic of the embodiment of the present application.
[0280] Comparative Examples 5 to 20 are all glass ceramics of the spinel system. However, since the composition of the glass ceramics and / or the surface stress distribution structure of the obtained reinforced glass ceramics do not meet the requirements of the present application, the value of the formula X related to the surface stress distribution is either too large or too small, and the scratch performance of the reinforced glass ceramics finally obtained is obviously inferior to the embodiment scheme that meets the requirements of the present application.
[0281] The above are only specific embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A reinforced glass ceramic, characterized in that: The reinforced glass ceramic comprises a main crystal phase of zinc aluminum spinel-magnesium aluminum spinel solid solution and a secondary crystal phase of zirconium oxide; The reinforced glass-ceramic has a compressive stress layer on the surface and tensile stress inside; the reinforced glass-ceramic satisfies: 1.50≤X≤4.70, preferably, 1.50≤X≤4.00, more preferably, 1.50≤X≤3.60; Wherein, CS_20 is the compressive stress value at a depth of 20 μm from the main surface of the strengthened glass-ceramic, in MPa; CS_30 is the compressive stress value at a depth of 30 μm from the main surface of the strengthened glass-ceramic, in MPa; CS_50 is the compressive stress value at a depth of 50 μm from the main surface of the strengthened glass-ceramic, in MPa; DOL_0 is the depth of the compressive stress layer of the strengthened glass-ceramic, in μm; DOL_K is K + Diffusion depth, in μm; In formula X, the data is substituted according to the above unit requirements to perform calculations and obtain calculation results. The units do not participate in the calculations.
2. The reinforced glass ceramic according to claim 1, characterized in that: The thickness t of the reinforced glass ceramic is 0.30 mm to 2.00 mm, preferably, the thickness t is 0.35 mm to 1.50 mm, more preferably, the thickness t is 0.40 mm to 1.00 mm; and / or, The reinforced glass ceramic is 2D, 2.5D, 3D or special-shaped.
3. The reinforced glass ceramic according to claim 1 or 2, characterized in that: The reinforced glass ceramics meet the following requirements: 70.00MPa≤CS_20≤250.00MPa, preferably, 75.00MPa≤CS_20≤245.00MPa, more preferably, 80.00MPa≤CS_20≤240.00MPa; and / or, 60.00MPa≤CS_30≤240.00MPa, preferably, 65.00MPa≤CS_30≤230.00MPa, more preferably, 70.00MPa≤CS_30≤221.00MPa; and / or, 50.00MPa≤CS_50≤210.00MPa, preferably, 55.00MPa≤CS_50≤200.00MPa, more preferably, 59.00MPa≤CS_50≤185.00MPa; and / or, 5.00 μm≤DOL_K≤25.00 μm, preferably, 7.00 μm≤DOL_K≤23.00 μm, more preferably, 9.00 μm≤DOL_K≤21.00 μm; and / or 0.17t≤DOL_0≤0.25t, preferably, 0.19t≤DOL_0≤0.25t, t is the thickness of the reinforced glass-ceramic; and / or, 65.00μm≤DOL_0≤240.00μm, preferably, 70.00μm≤DOL_0≤225.00μm, more preferably, 75.00μm≤DOL_0≤215.00μm.
4. The reinforced glass ceramic according to any one of claims 1 to 3, characterized in that The Vickers hardness of the reinforced glass ceramic is greater than or equal to 750 kgf / mm 2 Preferably, the Vickers hardness of the reinforced glass ceramic is greater than or equal to 800 kgf / mm 2 .
5. The reinforced glass ceramic according to any one of claims 1 to 4, characterized in that The reinforced glass ceramic is transparent in the visible light wavelength range. Preferably, when the thickness t of the reinforced glass ceramic is 0.40 mm to 1.00 mm, the transmittance of the reinforced glass ceramic for light with a wavelength of 550 nm is ≥85%, preferably ≥89%.
6. The reinforced glass ceramic according to any one of claims 1 to 5, characterized in that The composition at the center of the reinforced glass-ceramic, measured in mole percentage of oxides, comprises: SiO2: 40.00% ~ 50.00%, Al2O3: 20.00% ~ 30.00%, MgO: 3.00% ~ 8.00%, ZnO: 8.00% ~ 12.00%, BaO: 0% ~ 8.00%, CaO: 0% ~ 8.00% , ZrO2: 3.00% ~ 6.00%, Na2O: 2.00% ~ 10.00%, Li2O: 3.00% ~ 12.00%, K2O: 0% ~ 1.00%, Y2O3: 0% ~ 15.00% and La2O3: 0% ~ 15.00%.
7. The reinforced glass ceramic according to any one of claims 1 to 6, characterized in that The composition at the center of the reinforced glass-ceramic, measured in mole percentage of oxides, comprises: The molar percentage of SiO2 is 41.00% to 48.00%, preferably, the molar percentage of SiO2 is 42.00% to 47.00%; and / or, the molar percentage of Al2O3 is 22.00% to 29.00%, preferably, the molar percentage of Al2O3 is 25.00% to 28.00%; and / or, The molar percentage of MgO is 4.00% to 7.00%, preferably, the molar percentage of MgO is 5.00% to 6.00%; and / or, The molar percentage of ZnO is 8.50% to 11.50%, preferably, the molar percentage of ZnO is 9.00% to 11.00%; and / or, The molar percentage of BaO is 0.50% to 5.00%, preferably, the molar percentage of BaO is 1.00% to 4.00%; and / or, The molar percentage of CaO is 0% to 3.00%, preferably, the molar percentage of CaO is 0% to 1.50%; and / or, The molar percentage of ZrO2 is 3.00% to 5.00%, preferably, the molar percentage of ZrO2 is 3.10% to 4.00%; and / or, The molar percentage of Na2O is 2.50% to 8.00%, preferably, the molar percentage of Na2O is 3.00% to 6.00%; and / or, The molar percentage of Li2O is 3.20% to 10.00%, preferably, the molar percentage of Li2O is 3.50% to 6.00%; and / or, The molar percentage of Y2O3 is 0% to 5.00%, preferably, the molar percentage of Y2O3 is 0% to 1.00%; and / or, The molar percentage of La2O3 is 0% to 5.00%, and preferably, the molar percentage of La2O3 is 0% to 1.00%.
8. The reinforced glass ceramic according to any one of claims 1 to 7, characterized in that: The composition at the center of the reinforced glass-ceramic contains Y2O3 and / or La2O3, and the molar percentage of Y2O3 [Y2O3] and the molar percentage of La2O3 [La2O3] satisfy the following relationship: 0%<[Y2O3]+[La2O3]≤15.00%; preferably, 0%<[Y2O3]+[La2O3]≤5.00%, and more preferably, 0%<[Y2O3]+[La2O3]≤1.00%.
9. The reinforced glass ceramic according to any one of claims 1 to 8, characterized in that The composition at the center of the reinforced glass-ceramic satisfies that the value of [Y2O3]+[La2O3] is 0% or 0.38%.
10. The reinforced glass ceramic according to any one of claims 1 to 9, characterized in that: Measured in molar percentage of oxides, the composition of the reinforced glass-ceramic contains: no P2O5, and / or no B2O3, and / or no TiO2.
11. The reinforced glass ceramic according to any one of claims 1 to 12, characterized in that: The crystallinity of the reinforced glass ceramic is 30% to 55%, preferably 40% to 55%; and / or, In the reinforced glass-ceramic, the average crystal size does not exceed 20 nm, preferably 1 nm to 15 nm, and more preferably 3 nm to 8 nm.
12. The reinforced glass ceramic according to any one of claims 1 to 11, characterized in that: The reinforced glass ceramics meet the following requirements: CS_20 is 104.13 MPa, 83.36 MPa, 90.30 MPa, 190.30 MPa, 203.57 MPa, 101.89 MPa, 80.76 MPa, 111.28 MPa, 122.29 MPa, 142.68 MPa, 111.31 MPa, 162.64 MPa, 172.84 MPa, 238.66 MPa or 131.91 MPa; and / or, CS_30 is 95.34 MPa, 76.40 MPa, 78.38 MPa, 168.38 MPa, 187.61 MPa, 93.58 MPa, 73.53 MPa, 99.60 MPa, 110.58 MPa, 116.61 MPa, 103.81 MPa, 149.28 MPa, 149.98 MPa, 220.19 MPa or 124.52 MPa; and / or, CS_50 is 78.00 MPa, 62.67 MPa, 69.80 MPa, 99.80 MPa, 156.09 MPa, 77.19 MPa, 59.24 MPa, 79.80 MPa, 87.68 MPa, 66.34 MPa, 88.96 MPa, 123.29 MPa, 124.92 MPa, 184.10 MPa or 109.86 MPa; and / or, DOL_K is 12.20μm, 10.40μm, 9.60μm, 14.10μm, 13.30μm, 12.80μm, 11.90μm, 11. 50μm, 12.20μm, 10.10μm, 14.20μm, 12.50μm, 12.80μm, 16.30μm or 20.30μm; and / or, DOL_0 is 150.06μm, 151.72μm, 153.34μm, 159.04μm, 148.22μm, 156.93μm, 150.10μm, 153 .34μm, 153.68μm, 78.50μm, 181.56μm, 182.52μm, 181.75μm, 188.84μm or 214.61μm; and / or, The value of formula X is 1.90, 1.56, 2.35, 3.24, 2.07, 1.92, 1.91, 2.27, 2.21, 3.51, 1.79, 2.02, 3.43, 2.59 or 2.
18.
13. The reinforced glass ceramic according to any one of claims 1 to 12, characterized in that: The Vickers hardness of the reinforced glass ceramic is 850 kgf / mm 2 、810kgf / mm 2 、821kgf / mm 2 、824kgf / mm 2 、806kgf / mm 2 、812kgf / mm 2 、811kgf / mm 2 、823kgf / mm 2 、804kgf / mm 2 、816kgf / mm 2 、845kgf / mm 2 、814kgf / mm 2 、816kgf / mm 2 or 840kgf / mm 2 .
14. The reinforced glass ceramic according to any one of claims 1 to 13, characterized in that The composition at the center of the reinforced glass-ceramic, measured in mole percentage of oxides, comprises: The molar percentage of SiO2 is 45.31%, 45.76%, 46.29%, 45.13%, 45.85%, 46.76% or 42.52%; and / or, the molar percentage of Al2O3 is 25.80%, 27.03%, 26.36%, 25.70%, 26.10%, 26.62% or 27.36%; and / or, The molar percentage of MgO is 5.47%, 5.52%, 5.59%, 5.45%, 5.53%, 5.64% or 5.80%; and / or, The molar percentage of ZnO is 9.71%, 9.80%, 10.91%, 9.67%, 9.82%, 9.92%, 10.02% or 9.96%; and / or, The molar percentage of BaO is 1.16%, 1.17%, 0% or 3.47%; and / or, The molar percentage of CaO is 0% or 0.99%; and / or, The molar percentage of ZrO2 is 3.39%, 3.42%, 3.46%, 3.38%, 3.43%, 3.50% or 3.48%; and / or, The molar percentage of Na2O is 3.39%, 3.43%, 3.47%, 3.38%, 5.39%, 3.50% or 3.55%; and / or, The molar percentage of Li2O is 5.77%, 3.87%, 3.92%, 5.75%, 3.88%, 4.91%, 3.96% or 3.86%; and / or, the molar percentage of Y2O3 is 0% or 0.19%; and / or, The molar percentage of La2O3 is 0% or 0.19%.
15. The reinforced glass ceramic according to any one of claims 1 to 14, characterized in that The reinforced glass-ceramic, after the sand and stone scratch test, has a haze growth factor of less than 3.00, preferably less than 2.50, and more preferably less than 2.10, compared with the haze of the reinforced glass-ceramic before the sand and stone scratch test; Among them, the sand and gravel scratch test refers to placing the reinforced glass ceramics and 1 kg of silica sand in an oscillating abrader for scratch testing, the oscillation frequency of the oscillating abrader is 150 rpm, and the time of the sand and gravel scratch test is 10 min; the haze growth factor = (the final haze of the reinforced glass ceramics after the sand and gravel scratch test - the initial haze of the reinforced glass ceramics before the sand and gravel scratch test) / the initial haze of the reinforced glass ceramics before the sand and gravel scratch test.
16. A cover glass, characterized in that: The cover glass is made of the tempered glass ceramic according to any one of claims 1 to 15.
17. An electronic device, characterized in that: The electronic device comprises the reinforced glass-ceramic as described in any one of Claims 115.
18. The electronic device according to claim 17, characterized in that: The electronic device comprises a housing comprising the reinforced glass-ceramic according to any one of claims 1-15.
19. The electronic device according to claim 18, characterized in that: The housing comprises a display cover plate, and the display cover plate comprises the strengthened glass-ceramic according to any one of claims 1-15.
20. The electronic device according to claim 18 or 19, characterized in that: The housing comprises a rear cover comprising the reinforced glass-ceramic according to any one of claims 1-15.
21. The electronic device according to any one of claims 18 to 20, characterized in that: The electronic device further comprises a camera assembly, the housing comprises a camera protection cover, the camera protection cover is disposed on the camera assembly, and the camera protection cover comprises the reinforced glass ceramic according to any one of claims 1-15.
22. The electronic device according to any one of claims 17 to 21, characterized in that: The electronic device further comprises a middle frame, wherein the middle frame comprises the reinforced glass ceramic according to any one of claims 1 to 15.
23. A glass device, characterized in that: The glass device comprises the strengthened glass-ceramic according to any one of claims 1 to 15.
Citation Information
Patent Citations
Ion exchangeable, transparent gahnite-spinel glass ceramics with high hardness and modulus
CN111615500A
Transparent tempered glass ceramic with high stress depth and preparation method and application thereof
CN116409933A
Transparent colorless spinel microcrystalline glass and preparation and application thereof
CN118125715A
Spinel glass ceramic and application thereof
CN118125716A
Transparent spinel glass ceramic and preparation method therefor and use thereof
WO2023125035A1
Cited By
Chemically strengthened microcrystalline glass and preparation thereof
CN121672942A
Chemically strengthened microcrystalline glass and preparation thereof
CN121672942B
Precursor glass for preparing spinel glass ceramics
CN121698567A
Spinel glass ceramic and preparation method thereof
CN121698570A
Spinel microcrystalline glass and preparation method thereof
CN121698570B