Dealkalization solution for glass storage bottle and use method of dealkalization solution

By using a dealkali solution composed of oxalic acid, ammonium bifluoride and potassium fluoride in a glass storage bottle, hydrofluoric acid is slowly generated, which solves the problem of uncontrollable metal ion precipitation in traditional processes, reduces energy consumption and improves coating adhesion. effect.

CN118754452APending Publication Date: 2024-10-11CNBM RESEARCH INSTITUTE FOR ADVANCED GLASS MATERIALS GROUP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410976465.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The traditional inner surface treatment process of glass storage bottles cannot effectively control the precipitation of metal ions and impurities, and the hydrofluoric acid corrosion process is harmful to the human body and consumes high energy.

Method used

Using a dealkali solution composed of oxalic acid, ammonium bifluoride and potassium fluoride, the weak acid oxalic acid reacts with NH4HF2 and KF to slowly generate hydrofluoric acid, control the reaction rate, avoid high temperature treatment, and form a stable etching solution.

Benefits of technology

It effectively reduces the content of alkali metal ions on the inner surface of the glass storage bottle, improves the strength of the bonding force between the subsequent coating layer and the inner wall of the glass bottle, reduces energy consumption and experimental safety risks, and reduces waste gas and waste liquid emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a dealkalization solution for a glass storage bottle and a use method of the dealkalization solution. The dealkalization solution is characterized by comprising the following steps: (1) putting a glass bottle into deionized water for ultrasonic cleaning and then drying the glass bottle; (2) weighing the following raw materials in percentage by weight: 5-10% of oxalic acid, 5-15% of ammonium bifluoride, 1-3% of potassium fluoride and the balance of water, uniformly mixing, injecting the solution into a glass bottle, and treating at 20-25 DEG C for 10-20 minutes; and (3) washing the treated glass bottle with deionized water, then soaking the glass bottle with a sulfuric acid solution with the volume fraction of 1-3% for 3-5 minutes, finally washing the glass bottle with deionized water, and drying the glass bottle. The method has the advantages that strong acid is replaced by weak acid oxalic acid, hydrofluoric acid is slowly generated by reacting the weak acid oxalic acid with introduced NH4HF2 and KF, and the concentration of the hydrofluoric acid in the etching liquid is at a stable numerical value, so that the reaction rate is effectively controlled; the content percentage of alkali metal Na on the inner surface of the glass storage bottle treated by the method is reduced by 47% compared with that before dealkalization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass manufacturing and relates to a dealkalization solution for a glass storage bottle and a use method thereof. Background Art

[0002] Currently, the common methods for treating the inner surface of glass storage bottles mainly include frosting (de-alkali) treatment and siliconization treatment. However, due to the increasingly stringent requirements for ion precipitation control in glass storage bottles, the traditional frosting process can no longer meet the requirements for the precipitation of metal ions and other impurities on the inner surface. In addition, high-temperature heating is required during the frosting process, which consumes a lot of energy.

[0003] Hydrofluoric acid can open the glass network channels, which is beneficial to the precipitation of alkali metal ions. Hydrofluoric acid can also form micro-nano structures on the glass surface, which is beneficial to increase the bonding strength between the subsequent coating layer and the glass substrate. However, hydrofluoric acid is very harmful to the human body and the corrosion rate of the glass is uncontrollable. Summary of the invention

[0004] The purpose of the invention is to solve the problem that the corrosion process is difficult to control when the inner surface of a glass storage bottle is corroded by hydrofluoric acid, and to provide a dealkalization solution for a glass storage bottle and a use method thereof.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A dealkalizing solution for glass storage bottles is characterized in that it is made of the following raw materials in percentage by weight: 5%-10% oxalic acid, 5%-15% ammonium bifluoride and 1%-3% potassium fluoride, and the balance is water.

[0006] A dealkalizing solution for glass storage bottles is characterized in that it is made of the following raw materials in percentage by weight: 7%-9% oxalic acid, 7%-11% ammonium bifluoride and 1.2%-2.8% potassium fluoride, and the balance is water.

[0007] A dealkalizing solution for glass storage bottles is characterized in that it is made of the following raw materials in weight percentage: 7% to 11% oxalic acid content, 7% to 9% ammonium bifluoride content, 1.2% to 1.8% potassium fluoride, and the balance is water.

[0008] A method for using a dealkalizing solution for a glass storage bottle, characterized by comprising the following steps: (1) Place the glass bottle in deionized water for ultrasonic cleaning (25-35 minutes) and then dry it; (2) Weigh the following raw materials by weight and mix them: 5%-10% oxalic acid, 5%-15% ammonium bifluoride and 1%-3% potassium fluoride, with the balance being water. After mixing evenly, inject the solution into a glass bottle and treat at 20°C-25°C for 10-20 min. (3) Rinse the treated glass bottle with deionized water, then soak it in a 1% to 3% sulfuric acid solution for 3 to 5 min, finally rinse it with deionized water and dry it.

[0009] Furthermore, the glass bottle is made of the following raw materials in percentage by mass: SiO2 68-72%, Al2O3 1-1.15%, B2O3 0.45-0.48%, Na2O 13-13.2%, K2O 0.8-1%, MgO 2.3-2.8%, CaO 10-11%, BaO 0.8-1.2%, and Fe2O3 0.28-0.35%.

[0010] The present invention uses weak acid oxalic acid (C2H2O4•2H2O) instead of strong acid, and slowly generates hydrofluoric acid by reacting with the introduction of NH4HF2 and KF, so that the concentration of hydrofluoric acid in the etching solution is at a stable value, thereby effectively controlling the reaction rate. The percentage of alkali metal (taking Na as an example) content on the inner surface of the glass storage bottle treated by the present invention is reduced by 47% compared with that before dealkalization.

[0011] The advantages of the present invention are as follows: the present invention does not directly use hydrofluoric acid, but controls the rate of hydrofluoric acid generation by controlling the content of each component in the solution, thereby controlling the reaction rate. High temperature is not used in the whole process, which reduces energy consumption; and hydrofluoric acid is not directly used, which increases the safety of the experimental process and reduces the emission of waste gas and waste liquid in the production process. A rough micro-nano structure can be formed on the smooth inner wall surface of the glass bottle by hydrofluoric acid treatment, which is beneficial to improve the bonding force between the film layer and the inner wall of the glass bottle in the subsequent coating process. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 This is the SEM image of the inner surface of the glass bottle before being treated with dealkalizing solution; Figure 2 This is the SEM image of the inner surface of the glass bottle after treatment with dealkalizing solution. DETAILED DESCRIPTION

[0013] A method for using a dealkalizing solution for reducing the alkali ion content on the inner surface of a glass storage bottle, the specific implementation steps are as follows: The specifications of the glass storage bottle used in the present invention are as follows: the capacity of the glass bottle is 4L, the diameter of the bottle mouth is 35mm, the height is 340mm, and the composition mass percentage is as follows: SiO270%, Al2O31.12%, B2O30.45%, Na2O 13.16%, K2O 0.96%, MgO 2.5%, CaO 10.51%, BaO 1%, Fe2O30.30%. Example

[0014] Add 4L of deionized water into the glass bottle, place it at 25°C for 15 minutes, soak it in 3% sulfuric acid solution for 5 minutes, rinse it with deionized water, and dry it for testing. Example

[0015] Weigh 3 equal portions of 80g KF, 320g C2H2O4•2H2O, and 280g, 360g, and 440g NH4HF2, respectively, put them into 3 5000mL containers and mix them evenly with 4000ml deionized water; then pour the 3 mixed solutions into 3 glass bottles, place them at 25℃ for 15 minutes, soak them in 3% sulfuric acid solution for 5 minutes, and finally rinse them with deionized water, dry and test. Example

[0016] Weigh 360g NH4HF2, 320g C2H2O4•2H2O, and 48g, 80g, and 112g KF in three equal portions, put them into three 5000mL containers respectively, and mix them evenly with 4000ml deionized water; then pour the three mixed solutions into three glass bottles respectively, place them at 25℃ for 15 minutes, soak them in 3% sulfuric acid solution for 5 minutes, and finally rinse them with deionized water, dry and test. Example

[0017] Weigh 360g NH4HF2, 80g KF, and 280g, 320g, and 360g C2H2O4•2H2O in three equal portions, put them into three 5000mL containers respectively, and mix them evenly with 4000ml deionized water; then pour the three mixed solutions into three glass bottles respectively, place them at 25℃ for 15 minutes, soak them in 3% sulfuric acid solution for 5 minutes, and finally rinse them with deionized water, dry and test.

[0018] The EDS results of the inner surface of the glass storage bottle are shown in Table 1, and the SEM results of the glass storage bottle before and after treatment are shown in Table 1. Figure 1 shown.

[0019] Table 1 The percentage of alkali metal content on the inner surface of glass storage bottles after treatment with different ratio solutions

[0020] When the ammonium bifluoride content in the solution is 3%~10%, the oxalic acid content is 5%~10%, and the potassium fluoride content is 2%~5%, the alkali metal ion content on the inner surface of the glass storage bottle can be reduced by up to 47% compared with before dealkalization. After solution treatment, the inner surface of the glass storage bottle forms a rough surface, which is conducive to increasing the bonding strength between the subsequent coating and the film layer.

Claims

1. A dealkalization solution for glass storage bottles, Features The invention is prepared from the following raw materials in percentage by weight: 5%-10% oxalic acid, 5%-15% ammonium bifluoride and 1%-3% potassium fluoride, and the balance is water.

2. A dealkalization solution for glass storage bottles according to claim 1, Features The invention is prepared from the following raw materials in weight percentage: 7%-9% oxalic acid, 7%-11% ammonium bifluoride and 1.2%-2.8% potassium fluoride, and the balance is water.

3. The dealkalization solution for glass storage bottles according to claim 1, Features The invention is prepared from the following raw materials in weight percentage: 7% to 11% oxalic acid content, 7% to 9% ammonium bifluoride content, 1.2% to 1.8% potassium fluoride, and the balance is water.

4. A method for using a dealkalization solution for a glass storage bottle, Features The steps include: (1) Place the glass bottle in deionized water, ultrasonically clean it, and then dry it; (2) Weigh the following raw materials by weight and mix them: 5%-10% oxalic acid, 5%-15% ammonium bifluoride and 1%-3% potassium fluoride, with the balance being water. After mixing evenly, inject the solution into a glass bottle and treat at 20°C-25°C for 10-20 min. (3) Rinse the treated glass bottle with deionized water, then soak it in a 1% to 3% sulfuric acid solution for 3 to 5 min, finally rinse it with deionized water and dry it.

5. A method for using the dealkalization solution for glass storage bottles according to claim 4, Features The glass bottle is made of the following raw materials in percentage by mass: SiO 2 68-72%, Al 2 O 3 1-1.15%, B 2 O 3 0.45-0.48%, Na 2 O 13-13.2%, K 2 O 0.8-1%, MgO 2.3-2.8%, CaO 10-11%, BaO 0.8-1.2%, Fe 2 O 3 0.28-0.35%.

Citation Information

Cited By

  • Method for coating inner surface of glass container

    CN120040092A