Method for preparing dicalcium silicate clinker and carbon sequestration product by doping chromium ions as crystal form regulator
Preparation of dicalcium silicate clinker by doping chromium ions as a crystal form regulator, combined with the CO2 mineralization and curing process, solves the problem of low carbonization activity and insufficient mechanical properties of carbon fixation products, and achieves efficient carbonization and high carbon fixation capacity. , reduces costs and has dual environmental and economic benefits.
Patent Information
- Application Number
- CN202411021655.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-11
AI Technical Summary
Existing carbon sequestration products have slow CO2 mineralization rates, low carbon sequestration capacity, and insufficient mechanical properties, resulting in poor carbon emission reduction effects in the cement industry.
Dicalcium silicate clinker is prepared by doping chromium ions as a crystal modifier to control the carbonization characteristics. The CO2 mineralization curing process is used, combined with parameter optimization during the sintering and carbonization processes, to improve the carbonization activity and mechanical properties of carbon-fixed products.
It achieves efficient carbonization of carbon-fixing products, improves carbon-fixing capacity and mechanical properties, reduces maintenance costs, has a simple process and does not release CO2, and has dual environmental and economic benefits.
Smart Images

Figure CN118754467A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon-fixing cementitious materials, and in particular relates to a method for preparing dicalcium silicate clinker and carbon-fixing products by doping with chromium ions as a crystal form regulator. Background Art
[0002] Against the backdrop of increasingly severe global warming, excessive carbon dioxide emissions have attracted widespread attention worldwide. The cement industry is recognized as a major emitter of carbon dioxide, contributing 6%-8% of total carbon emissions, so it is urgent to promote carbon emission reduction in the cement industry. Taking advantage of the carbonization reaction of calcium silicate minerals with carbon dioxide, the development and utilization of carbon-fixing products with low-calcium calcium silicate as the main mineral phase and high carbonization activity has become one of the most promising methods to reduce carbon emissions in the cement industry.
[0003] In recent years, carbon-fixing products made of carbonated cementitious materials mainly composed of low-calcium silicate mineral γ-C2S have attracted widespread attention and extensive research from scholars at home and abroad because of their higher carbonization activity and unique advantages of self-powdering, which can effectively reduce the energy consumption of grinding. However, there are still many problems to be solved for its carbon-fixing products, such as: its low early carbonization activity increases the maintenance cost to a certain extent; and its carbon fixation capacity is limited. After a period of carbonization reaction, the densification of the carbonization products generated by the reaction hinders the inward diffusion of carbon dioxide gas, resulting in the difficulty of improving the strength of carbon-fixing products in the later stage. In order to further improve the carbonization performance of carbon-fixing products, the methods currently commonly used in China are: first, increasing the carbon dioxide concentration of the carbonization reaction; second, increasing the pressure of the carbonization reaction, but these two methods will greatly increase the maintenance cost, and the process is complicated, which is not conducive to energy conservation and emission reduction.
[0004] Although there are methods for modifying γ-C2S by doping with metal ions, they still have their own problems: Patent CN111393049A discloses a method for activating and modifying γ-C2S, which modifies γ-C2S by sintering with externally doped barium ions and magnesium ions, thereby preparing γ-C2S with high specific surface area and high carbonization activity, further improving the performance of carbonized products, but this method does not significantly improve the carbon fixation capacity and mechanical properties.
[0005] The present invention achieves the regulation of the carbonization characteristics of the carbon-fixing product by regulating parameters such as the type and dosage of chromium ions, and performs CO2 mineralization curing on the product. The mechanical properties of the high-efficiency carbon-fixing product are tested in accordance with GB / T50081-2002 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the carbonization degree of the product is evaluated by thermogravimetric analysis. Summary of the invention
[0006] In response to the problems raised by the background technology, the purpose of the present invention is to provide a method for preparing dicalcium silicate clinker and carbon-fixing products by doping with chromium ions as a crystal regulator, so as to solve the problems of slow CO2 mineralization rate, low carbon fixation capacity, and insufficient development of mechanical properties of existing carbon-fixing products.
[0007] In order to achieve the above object, the present invention specifically adopts the following technical solutions: The present invention provides a method for preparing a dicalcium silicate carbon-fixing product by doping chromium ions as a crystal form regulator, comprising the following steps: S1. Evenly mix the chromium ion crystal form regulator with the calcium raw material and the silicon raw material, add water and ball mill to obtain a mixed slurry, and dry to obtain a raw material; S2, mixing the raw material obtained in S1 with anhydrous ethanol, stirring evenly and pressing into a green body, and sintering and cooling the green body to obtain dicalcium silicate clinker; S3. Add water to the clinker obtained in S2 and press it into a preformed matrix, and then carbonize it to obtain a carbon-fixed product.
[0008] Furthermore, the chromium ion crystal form regulator in S1 is at least one of Cr2O3, CrO3, Cr(OH)3, Cr-contaminated soil or contaminated water.
[0009] Furthermore, the calcium raw material in S1 is at least one of Ca(OH)2, CaCO3, carbide slag, waste marble, and waste cement stone.
[0010] Furthermore, the siliceous raw material in S1 is at least one of SiO2, sandstone, copper tailings, waste glass, and rice husk ash.
[0011] Furthermore, the molar ratio of calcium to silicon in the mixture of S1 chromium ion crystal form regulator and calcium raw material and silicon raw material is 0.6-4.0, and the dosage of chromium ion crystal form regulator is 0.1%-5% of the total mass of calcium raw material and silicon raw material.
[0012] Furthermore, the liquid-to-solid ratio of the water-added ball milling in S1 is (1-200):1, the ball milling speed is 100-1000 rpm, and the ball milling time is 1-48 h.
[0013] Furthermore, the liquid-solid ratio of the S2 raw material mixed with anhydrous ethanol is 0.1-0.8, and the molding pressure of the pressed body is 10-100 MPa.
[0014] Furthermore, the sintering conditions of S2 are: heating rate of 5-10°C / min, sintering temperature of 1200-1500°C, and holding time of 1-12 h.
[0015] Furthermore, the water-to-solid ratio of the S3 clinker with water is 0.10-0.30, the preform matrix molding pressure is 2-30 MPa, the CO2 concentration of the carbonization reaction is 10%-100%, and the humidity is 30%-98%.
[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) The preparation of colored carbon-fixing products is realized, and the color is stable and not easy to change or fall off after high temperature, which is of great significance for expanding the application of colored carbon-fixing products.
[0017] (2) During the sintering process, chromium ions stabilize the β-C2S crystals and inhibit the β-C2S crystal phase transformation. By adjusting the ratio of dicalcium silicate (i.e., γ-C2S and β-C2S), the carbonization activity and carbon fixation capacity of the carbon-fixing products are effectively improved from the source, thereby improving the mechanical properties. The cost is low and the process is simple.
[0018] (3) Most previous studies have focused on carbon-fixing cementitious materials under a single γ-C2S or β-C2S mineral phase. The present invention proposes a new idea of synergistic carbon fixation in carbon-fixing products based on the coexistence of two calcium silicate mineral phases, γ-C2S and β-C2S. In the first stage, the carbonization activation energy of β-C2S is low, so the carbonization reaction can be carried out first. The carbonization releases heat to promote the hydration reaction of β-C2S. The hydration of β-C2S generates CSH gel, which acts as a cementing agent together with the silica gel generated by γ-C2S, making the calcium carbonate skeleton tightly connected. In the second stage, CSH continues to carbonize to form calcium carbonate and silica gel, with a denser structure, to obtain a carbon-fixing product.
[0019] (4) The present invention does not release CO2 during the clinker sintering process, and the clinker can also seal a large amount of CO2, while realizing the resource utilization of heavy metal ions and effectively solidifying heavy metal ions, providing a new idea for establishing CO2 emission reduction and heavy metal ion safe disposal with both environmental and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a graph of the compressive strength of Examples 1-3 and Comparative Example 1.
[0021] Figure 2 The graphs and X-ray diffraction patterns of the dicalcium silicate clinker of Examples 1-3 and Comparative Example 1 are shown.
[0022] Figure 3 The X-ray diffraction patterns of the carbon-fixing products of Examples 1-3 and Comparative Example 1 are shown.
[0023] Figure 4 The microscopic morphology of the carbonized products of Example 2 and Comparative Example 1 after carbonization for 1 h and 24 h.
[0024] Figure 5It is a curve diagram of the pH value change of the clinker suspension of Examples 1-3 and Comparative Example 1 before and after the carbonization reaction.
[0025] Figure 6 TGA curves of the carbon-fixing products of Examples 1-3 and Comparative Example 1. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0028] Example 1 A method for preparing dicalcium silicate clinker and carbon-fixing products by using chromium ion doping as a crystal form regulator comprises the following steps: (1) 1 part of chromium trioxide, 71.2 parts of calcium hydroxide and 28.8 parts of silicon dioxide were mixed and stirred evenly, then mixed with deionized water and stirred again for a certain period of time to allow the mixture to be fully dispersed in the water. The mixture was then poured into a ball mill for mechanical ball milling, and finally dried at 105°C, wherein the liquid-to-solid ratio was 2:1, the calcium-to-silicon ratio was 2.0, the ball mill speed was set to 250 r / min, and the duration was 24 h, thereby obtaining a raw material.
[0029] (2) The raw material and anhydrous ethanol were mixed evenly (liquid-to-solid ratio was 0.2), and then pressed into a green body at a pressure of 30 MPa. The green body was then dried and placed in a high-temperature box furnace. The temperature was raised to 1400°C at a rate of 10°C / min and kept at that temperature for 3 h. After cooling to room temperature, the green body was taken out to obtain CO2 mineralized clinker, which was ground and passed through a 75 µm sieve.
[0030] (3) The clinker was pressed into a φ 20 mm × 20 mm cylindrical specimen with a water-solid ratio of 0.15 and a specimen molding pressure of 10 MPa. The holding time was 1 min and the mechanical properties were tested after carbonization for 1 h and 24 h (CO2 concentration was 99% and humidity was 98%).
[0031] (4) The mechanical properties of carbon-fixed products were tested in accordance with GB / T 50081-2002 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the degree of carbonization was tested by thermogravimetric analysis.
[0032] Example 2 A method for preparing dicalcium silicate clinker and carbon-fixing products by using chromium ion doping as a crystal form regulator comprises the following steps: (1) 1.5 parts of chromium trioxide, 71.2 parts of calcium hydroxide and 28.8 parts of silicon dioxide are mixed and stirred evenly, then mixed with deionized water and stirred again for a certain period of time to allow the mixture to be fully dispersed in the water. The mixture is then poured into a ball mill for mechanical ball milling, and finally dried at 105°C, wherein the liquid-to-solid ratio is 2:1, the calcium-to-silicon ratio is 2.0, the ball mill speed is set to 250 r / min, and the duration is 24 h, thereby obtaining a raw material.
[0033] (2) The raw material and anhydrous ethanol were mixed evenly (liquid-to-solid ratio was 0.2), and then pressed into a green body at a pressure of 30 MPa. The green body was then dried and placed in a high-temperature box furnace. The temperature was raised to 1400°C at a rate of 10°C / min and kept at that temperature for 3 h. After cooling to room temperature, the green body was taken out to obtain CO2 mineralized clinker, which was ground and passed through a 75 µm sieve.
[0034] (3) The clinker was pressed into a φ 20 mm × 20 mm cylindrical specimen with a water-solid ratio of 0.15 and a specimen molding pressure of 10 MPa. The holding time was 1 min and the mechanical properties were tested after carbonization for 1 h and 24 h (CO2 concentration was 99% and humidity was 98%).
[0035] (4) The mechanical properties of carbon-fixed products were tested in accordance with GB / T 50081-2002 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the degree of carbonization was tested by thermogravimetric analysis.
[0036] Example 3 A method for preparing dicalcium silicate clinker and carbon-fixing products by using chromium ion doping as a crystal form regulator comprises the following steps: (1) 2 parts of chromium trioxide, 71.2 parts of calcium hydroxide and 28.8 parts of silicon dioxide are mixed and stirred evenly, then mixed with deionized water and stirred again for a certain period of time to allow the mixture to be fully dispersed in the water. The mixture is then poured into a ball mill for mechanical ball milling, and finally dried at 105°C, wherein the liquid-to-solid ratio is 2:1, the calcium-to-silicon ratio is 2.0, the ball mill speed is set to 250 r / min, and the duration is 24 h, thereby obtaining a raw material.
[0037] (2) The raw material and anhydrous ethanol were mixed evenly (liquid-to-solid ratio was 0.2), and then pressed into a green body at a pressure of 30 MPa. The green body was then dried and placed in a high-temperature box furnace. The temperature was raised to 1400°C at a rate of 10°C / min and kept at that temperature for 3 h. After cooling to room temperature, the green body was taken out to obtain CO2 mineralized clinker, which was ground and passed through a 75 µm sieve.
[0038] (3) The clinker was pressed into a φ 20 mm × 20 mm cylindrical specimen with a water-solid ratio of 0.15 and a specimen molding pressure of 10 MPa. The holding time was 1 min and the mechanical properties were tested after carbonization for 1 h and 24 h (CO2 concentration was 99% and humidity was 98%).
[0039] (4) The mechanical properties of carbon-fixed products were tested in accordance with GB / T 50081-2002 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the degree of carbonization was tested by thermogravimetric analysis.
[0040] Comparative Example 1 A method for preparing dicalcium silicate clinker and carbon-fixing products by using chromium ion doping as a crystal form regulator comprises the following steps: (1) 71.2 parts of calcium hydroxide and 28.8 parts of silicon dioxide were mixed and stirred evenly, and then mixed with deionized water and stirred again for a certain period of time to allow the mixture to be fully dispersed in the water. The mixture was then poured into a ball mill for mechanical ball milling, and finally dried at 105° C., wherein the liquid-to-solid ratio was 2:1, the calcium-silicon ratio was 2.0, the ball mill speed was set to 250 r / min, and the duration was 24 hours, to obtain a raw material.
[0041] (2) The raw material and anhydrous ethanol were mixed evenly (liquid-to-solid ratio was 0.2), and then pressed into a green body at a pressure of 30 MPa. The green body was then dried and placed in a high-temperature box furnace. The temperature was raised to 1400°C at a rate of 10°C / min and kept at that temperature for 3 h. After cooling to room temperature, the green body was taken out to obtain CO2 mineralized clinker, which was ground and passed through a 75 µm sieve.
[0042] (3) The clinker was pressed into a φ 20 mm × 20 mm cylindrical test block with a water-solid ratio of 0.15 and a test block molding pressure of 10 MPa. The pressure holding time was 1 min. After carbonization for 1 h and 24 h (CO2 concentration was 99% and humidity was 98%), its mechanical properties were tested.
[0043] (4) The mechanical properties of carbon-fixed products were tested in accordance with GB / T 50081-2002 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the degree of carbonization was tested by thermogravimetric analysis.
[0044] The results show that the carbon fixation product obtained by the method of the present invention does not release CO2 during the preparation process, and has the characteristics of fast mineralization rate, high carbon fixation capacity and rapid development of mechanical properties after being driven by CO2 mineralization. Figure 1 And as shown in Table 1.
[0045] Table 1 Carbonization degree table
[0046] from Figure 1The compressive strength test results show that the carbon-fixing products fired with CrO3 have higher compressive strength after carbonization. Compared with the carbon-fixing products fired without CrO3 in Comparative Example 1, when the CrO3 content is 1.5%, the compressive strength of the clinker reaches 110 MPa after carbonization for 1 h, which is about 60% higher than that after carbonization for 24 h. The compressive strength is as high as 137 MPa, which is about 80% higher than that of the carbon-fixing products fired without CrO3 in Comparative Example 1. 6+ It has a significant effect on improving the mechanical properties of carbon-fixed products.
[0047] Figure 2 The dicalcium silicate clinker diagram and X-ray diffraction spectrum of Examples 1-3 and Comparative Example 1. It can be seen from the dicalcium silicate clinker diagram that with the addition of CrO3, the color of the clinker changes significantly and turns green, and with the increase of the CrO3 dosage, the green color gradually deepens, and the proportion of the solid part gradually increases. It can be seen from the X-ray diffraction spectrum that when the CrO3 dosage is 0%, the mineral phase of the burnt clinker is mainly γ-C2S, and with the increase of the CrO3 dosage, the β-C2S of the clinker mineral phase gradually increases. When the CrO3 dosage is 2%, the mineral phase of the burnt clinker is mainly β-C2S, and the γ-C2S of the clinker mineral phase basically disappears. This shows that the CrO3 in the present invention is not as effective as the CrO3 in the present invention. 6+ During the sintering process, it stabilizes the β-C2S crystals and prevents the transformation of β-C2S to γ-C2S.
[0048] Figure 3 The X-ray diffraction patterns of the carbon-fixing products of Examples 1-3 and Comparative Example 1 after carbonization for 1 h and 24 h are shown in the figure. It can be seen from the figure that calcium carbonate is generated by the carbonization reaction, which is because CO2 dissolves in water to form CO3 2- , and then react with the alkali metal (i.e. CaO) component in the mineral. From the diffraction peak of calcium carbonate, the calcium carbonate crystal form after carbonization of γ-C2S and β-C2S is mainly calcite. Calcium carbonate is the main source of compressive strength of carbon-fixed products.
[0049] Figure 4 The microscopic morphology of Example 2 and Comparative Example 1. It can be seen from the figure that both of them produce well-crystallized calcite-type calcium carbonate at the early carbonization of 1 h. For the comparative example clinker, the carbonization product is not tightly bonded to other components, and the entire structure is loose and porous. The clinker with a CrO3 content of 1.5% has a dense structure after carbonization for 1 h. The silica gel generated by γ-C2S and the CSH gel generated by β-C2S use mechanical bite bonding to tightly bond the calcium carbonate particles together. This phenomenon is more obvious after carbonization for 24 h. The clinker with a CrO3 content of 1.5% generates a large amount of calcium carbonate after carbonization for 24 h and continuously fills the pores, and its structure is more dense.
[0050] Figure 5 The pH value change curve of Examples 1-3 and Comparative Example 1 is shown in the figure. It can be seen from the figure that before the introduction of CO2, the pH value of the clinker increases rapidly, but the pH difference is not large. After 5 minutes of introduction of CO2, the free silicate and Ca in the clinker suspension with different dosages increase. 2+ Will react with dissolved CO3 2- The reaction generates CaCO3 and silica gel, and the pH drops rapidly and then tends to stabilize. The pH of the three groups of clinkers with CrO3 added is always higher than that of the control group, and the ion dissolution rate of the 1.5% addition is significantly faster than that of other additions, and the carbonization activity is the highest, indicating that CrO3 6+ It has a good effect on improving the carbonization reaction activity of carbon-fixing products.
[0051] Figure 6 Table 1 and Table 2 are the TGA curves and carbonization degree tables of the carbon-fixing products of Examples 1-3 and Comparative Example 1, respectively. It can be seen that the carbon-fixing product with a CrO3 content of 1.5% has a carbonization degree of 46.82% in 1 h and a carbonization degree of 59.17% in 24 h. When the CrO3 content is appropriate, as the carbonization time increases from 1 h to 24 h, the carbonization degree continues to increase, while when no CrO3 is added in the comparative example, the carbonization degree from 1 h to 24 h is almost unchanged. This shows that the CrO3 content in the present invention is 1.5%. 6+ It has a significant effect on improving the carbon fixation capacity of carbon fixation products.
[0052] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator, characterized in that: The steps include: S1. Evenly mix the chromium ion crystal form regulator with the calcium raw material and the silicon raw material, add water and ball mill to obtain a mixed slurry, and dry to obtain a raw material; S2, mixing the raw material obtained in S1 with anhydrous ethanol, stirring evenly and pressing into a green body, and sintering and cooling the green body to obtain dicalcium silicate clinker; S3. Add water to the clinker obtained in S2 and press it into a preformed matrix, and then carbonize it to obtain a carbon-fixed product.
2. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: S1 The chromium ion crystal form regulator is at least one of Cr2O3, CrO3, Cr(OH)3, Cr-contaminated soil or contaminated water.
3. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: S1 The calcium raw material is at least one of Ca(OH)2, CaCO3, carbide slag, waste marble and waste cement stone.
4. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: S1 The siliceous raw material is at least one of SiO2, sandstone, copper tailings, waste glass, and rice husk ash.
5. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: The molar ratio of calcium to silicon in the mixture of S1 chromium ion crystal form regulator and calcium raw material and silicon raw material is 0.6-4.0, and the dosage of chromium ion crystal form regulator is 0.1%-5% of the total mass of calcium raw material and silicon raw material.
6. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: The liquid-to-solid ratio of the water-added ball mill in S1 is (1-200):1, the ball mill speed is 100-1000 rpm, and the ball mill time is 1-48 h.
7. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: The liquid-to-solid ratio of the S2 raw material mixed with anhydrous ethanol is 0.1-0.8, and the molding pressure of the pressed body is 10-100 MPa.
8. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: The sintering conditions of S2 are: heating rate of 5-10℃ / min, firing temperature of 1200-1500℃, and holding time of 1-12h.
9. The method for preparing dicalcium silicate carbon-fixing products by using chromium ion doping as a crystal form regulator according to claim 1, characterized in that: The water-to-solid ratio of S3 clinker with water is 0.10-0.30, the preform matrix molding pressure is 2-30 MPa, the CO2 concentration of the carbonization reaction is 10%-100%, and the humidity is 30%-98%.
Citation Information
Patent Citations
Activation modification method of gamma-C2S
CN111393049A