Corrosion-resistant digital aggregate based on three-dimensional barrier as well as preparation and application of corrosion-resistant digital aggregate
By covering the radio frequency chip and concrete aggregate with two layers of protective layers, the problem of radio frequency chips being easily corroded in concrete is solved, the stability and compressive strength of signal transmission are achieved, and it is suitable for identification management and quality traceability of concrete components. .
Patent Information
- Application Number
- CN202411005792.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-25
AI Technical Summary
In the existing technology, radio frequency chips are susceptible to corrosion in concrete components, resulting in a decrease in signal transmission performance. Especially in underground water corrosion environments, this seriously affects the identification and traceability functions of concrete components.
Corrosion-resistant digital aggregate based on three-dimensional barrier is used, and the radio frequency unit and the aggregate body are covered with two protective layers. The first protective layer is composed of polyimide, fluorinated ethylene propylene copolymer and other materials, and the second The protective layer is composed of carbon mineralized materials, sodium tetraborate and other materials, which protect corrosive substances at the physical and chemical levels respectively, forming a stable internal environment.
It effectively improves the anti-corrosion performance of the radio frequency chip, maintains the stability of signal transmission, and avoids the degradation of signal transmission performance caused by external corrosive substances. It is suitable for label management and quality traceability of concrete products and cast-in-place structures.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of intelligent building materials, and in particular to a corrosion-resistant digital aggregate based on three-dimensional barrier and the preparation and application thereof. Background Art
[0002] At present, in the cement concrete prefabricated parts industry, most companies still use manual inventory methods to mark and inventory prefabricated parts. Faced with a large number of prefabricated parts, manual marking and inventorying are labor-intensive, inefficient, and prone to errors. Some companies also choose to paste QR codes on the surface of prefabricated parts to achieve information management. However, due to the complex service environment, the QR codes are easily damaged and fall off, resulting in little effect.
[0003] Radio frequency technology, as a method of communicating using electromagnetic waves, can be used to identify and trace concrete structures or components. However, when the RF chip is embedded in concrete for use, the shielding effect of concrete on electromagnetic waves will significantly reduce the signal transmission distance; at the same time, as the service life of concrete increases, external corrosive substances can diffuse into the concrete through cracks or pores and corrode the RF chip. Concrete components used in underground spaces, such as concrete pipes and segments, will also significantly reduce the life of their internal RF chips when corroded by groundwater, thereby significantly reducing their signal transmission performance, which will seriously affect the identification and traceability functions of concrete components.
[0004] Therefore, it is necessary to provide a solution to improve the anti-corrosion performance of RF chips. Summary of the invention
[0005] In view of this, the present application provides a corrosion-resistant digital aggregate based on three-dimensional barrier and its preparation and application, which are used to solve the problem of how to improve the anti-corrosion performance of radio frequency chips.
[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions: In the first aspect, the present application provides a corrosion-resistant digital aggregate based on three-dimensional barrier, including a mineralized aggregate blank and a first protective layer coated on the surface of the mineralized aggregate blank; the aggregate blank includes a radio frequency unit and a second protective layer coated on the radio frequency unit; the raw material of the first protective layer includes a first protective agent, and the first protective agent includes one or more of polyimide, fluorinated ethylene propylene copolymer, and soluble polytetrafluoroethylene; the raw material of the second protective layer includes a carbon mineralized material, a reinforcing agent, and a second protective agent, and the second protective agent includes one or more of sodium tetraborate, sodium silicate, and sodium aluminate.
[0007] Preferably, the mass ratio of the radio frequency unit, the carbon mineralization material, the first protective agent, the second protective agent, and the reinforcing agent is 1:8-64:1-21:2-40:1-11.
[0008] Preferably, the carbon mineralization material includes one or more of tricalcium silicate, γ-type dicalcium silicate, β-type dicalcium silicate, monocalcium silicate, tricalcium disilicate, calcium hydroxide, magnesium hydroxide, calcium oxide, and magnesium oxide; and the particle size of the carbon mineralization material is 75-150 μm.
[0009] Preferably, the enhancer includes one or more of chitosan, sodium alginate, polyethylene glycol, and polyvinyl alcohol.
[0010] Preferably, the radio frequency unit includes a radio frequency chip and a radio frequency antenna connected to the radio frequency chip.
[0011] In a second aspect, the present application provides a method for preparing a corrosion-resistant digital aggregate based on steric barrier, comprising the following steps: S1. mixing the carbon mineralization material, the second protective agent, the reinforcing agent and water to obtain a mixture; S2. In a mold, the RF unit is embedded in the mixture and pressed to obtain an aggregate body; S3. Under a carbon dioxide atmosphere, the aggregate body is mineralized to obtain a mineralized aggregate body; S4. Apply the first protective agent to the surface of the mineralized aggregate body, and after drying to form a film, a corrosion-resistant digital aggregate based on three-dimensional barrier is obtained.
[0012] Preferably, in step S2, the pressing pressure is 10-60 MPa.
[0013] Preferably, in step S3, the partial pressure of carbon dioxide is 0.1-0.3 MPa, the volume concentration of carbon dioxide is 20-99.9%, the mineralization temperature is 5-90° C., and the mineralization time is 12-48 h.
[0014] Preferably, in step S4, the coating thickness is 0.1-0.5 mm and the film forming time is 1-3 min.
[0015] In a third aspect, the present application provides an application of a corrosion-resistant digital aggregate based on three-dimensional barrier in the field of concrete components and / or cast-in-place structures.
[0016] The beneficial effects of the present application are as follows: the present application protects the digital aggregate at the physical and chemical levels respectively through two layers of protection measures, cooperates with each other, and synergistically blocks corrosive substances, maintains a relatively stable pH value in the internal environment, and protects the carbonization reaction products, thereby ensuring the stability of the digital aggregate strength signal transmission; when the digital aggregate is used for identification management and quality traceability of concrete products, prefabricated components or cast-in-place structures, the problem of reduced digital aggregate signal transmission performance caused by external corrosive substances can be effectively avoided. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0018] The present application provides a corrosion-resistant digital aggregate based on three-dimensional barrier, comprising a mineralized aggregate blank and a first protective layer coated on the surface of the mineralized aggregate blank; the aggregate blank comprises a radio frequency unit and a second protective layer coated on the radio frequency unit; the raw material of the first protective layer comprises a first protective agent, and the first protective agent comprises one or more of polyimide, fluorinated ethylene propylene copolymer, and soluble polytetrafluoroethylene; the raw material of the second protective layer comprises a carbon mineralized material, a reinforcing agent, and a second protective agent, and the second protective agent comprises one or more of sodium tetraborate, sodium silicate, and sodium aluminate.
[0019] In the present application, a digital aggregate is prepared by forming a carbonate mineral encapsulated radio frequency chip through the mineralization reaction of a carbon mineralized material; wherein, a first protective agent is used on the surface of the digital aggregate, has high density, good hydrophobicity, and strong corrosion resistance, and can physically block the invasion of corrosive substances in the external environment into the digital aggregate, reducing the probability of contact with corrosive substances, and serving as the first barrier of the digital aggregate; a second protective agent is added to the inside of the digital aggregate for use, and the hydroxyl radicals generated by its hydrolysis can react with the corrosive substances that break through the first protective agent, serving as the second barrier of the digital aggregate; the first protective agent and the second protective agent successively protect the digital aggregate at the physical and chemical levels respectively, cooperate with each other, and synergistically block, maintain the internal environment pH relatively stable, and protect the carbonization reaction products, thereby ensuring the stability of the digital aggregate intensity signal transmission.
[0020] In the present application, the first protective agent can be made into a solution with strong adhesion, good film-forming performance, strong hydrophobicity, dense structure, and excellent corrosion resistance. After film formation, it can effectively block corrosive substances, protect the digital aggregate at the physical level, and reduce the probability of contact between corrosive substances and digital aggregates; the second protective agent can hydrolyze to form weak acids and hydroxides, and promptly capture corrosive substances that break through the first protective layer and penetrate into the digital aggregate, maintaining the relative stability of the pH inside the digital aggregate, and the weak acid is weaker than carbonic acid, does not react with the digital aggregate, and the dielectric constant is close to that of the carbon mineralization product, which has little effect on the signal transmission performance of the digital aggregate.
[0021] In some embodiments, the mass ratio of the radio frequency unit, the carbon mineralization material, the first protective agent, the second protective agent, the reinforcing agent, and water is 1:8-64:1-21:2-40:1-11:1-21.
[0022] In some embodiments, the carbon mineralized material includes one or more of tricalcium silicate, γ-type dicalcium silicate, β-type dicalcium silicate, monocalcium silicate, tricalcium disilicate, calcium hydroxide, magnesium hydroxide, calcium oxide, and magnesium oxide; and the particle size of the carbon mineralized material is 75-150 μm.
[0023] In some embodiments, the reinforcing agent includes one or more of chitosan, sodium alginate, polyethylene glycol, and polyvinyl alcohol. The reinforcing agent can induce the generation of more carbonate minerals in the mineralization reaction, fill the pores of the digital aggregate, improve the compatibility of the digital aggregate with concrete materials, and increase the compressive strength of the digital aggregate.
[0024] In some embodiments, the RF unit includes a RF chip and a RF antenna connected to the RF chip. Under the stimulation of the signal collector, the internal information of the RF chip can be sent by the RF antenna and received by the signal collector. The operating frequency of the signal collector includes 30-300kHz low frequency, 3-30MHz high frequency and 433-950MHz ultra-high frequency.
[0025] In a second aspect, the present application provides a method for preparing a corrosion-resistant digital aggregate based on steric barrier, comprising the following steps: S1. mixing the carbon mineralization material, the second protective agent, the reinforcing agent and water to obtain a mixture; S2. In the mold, the RF unit is embedded in the mixture, and the aggregate body is obtained by pressing; the specific embedding process is to fill the mixture into the half-height position of the mold, and place the RF unit in the center of the mold, and continue to fill the mixture until it is filled; S3. Under a carbon dioxide atmosphere, the aggregate body is mineralized to obtain a mineralized aggregate body; S4. Apply the first protective agent to the surface of the mineralized aggregate body, and after drying to form a film, a corrosion-resistant digital aggregate based on three-dimensional barrier is obtained.
[0026] In some embodiments, the aggregate blank includes regular shapes and / or irregular shapes according to the morphology of the mold, and the regular shapes include but are not limited to cylinders, squares, and strips.
[0027] Preferably, in step S2, the pressing pressure is 10-60 MPa.
[0028] Preferably, in step S3, the partial pressure of carbon dioxide is 0.1-0.3 MPa, the volume concentration of carbon dioxide is 20-99.9%, the mineralization temperature is 5-90° C., and the mineralization time is 12-48 h.
[0029] Preferably, in step S4, the coating thickness is 0.1-0.5 mm and the film forming time is 1-3 min.
[0030] In a third aspect, the present application provides an application of a corrosion-resistant digital aggregate based on three-dimensional barrier in the field of concrete components and / or cast-in-place structures.
[0031] The corrosion-resistant digital aggregate design and preparation method based on three-dimensional barrier proposed in the present invention has a simple technical principle and obvious effect. The digital aggregate prepared based on this method can be widely used on the surface or inside of concrete products, prefabricated components or cast-in-place structures, and has excellent corrosion resistance.
[0032] The present solution is further described below through specific embodiments.
[0033] Example 1 A corrosion-resistant digital aggregate based on three-dimensional barrier comprises a mineralized aggregate blank and a first protective layer coated on the surface of the mineralized aggregate blank; the aggregate blank comprises a radio frequency unit and a second protective layer coated on the radio frequency unit; the raw material of the first protective layer comprises a first protective agent, which is polyimide; the raw material of the second protective layer is a mixture of γ-type dicalcium silicate, chitosan and sodium tetraborate with a particle size of 150 μm; the radio frequency unit comprises a radio frequency chip and a radio frequency antenna connected to the radio frequency chip; the usage of the radio frequency unit, γ-type dicalcium silicate, polyimide, sodium tetraborate, chitosan and water are 1 part, 36 parts, 11 parts, 21 parts, 6 parts and 11 parts respectively.
[0034] The method for preparing corrosion-resistant digital aggregate based on steric barrier comprises the following steps: S1. mixing chitosan with water to form a mixed solution, and mixing γ-type dicalcium silicate and sodium tetraborate with the mixed solution to obtain a mixture; S2. Fill the mixture into the mold at half height, place the RF unit in the center of the mold, continue to fill the mixture until it is full, and prepare the aggregate blank by pressing; the pressing pressure is 30MPa, repeat the above steps to prepare 6 aggregate blanks; S3. The aggregate body is placed in a carbon dioxide atmosphere for mineralization, the mineralization pressure is 0.2MPa, the temperature is 25°C, the relative humidity is 50%, the carbon dioxide volume concentration is 99.9%, the duration is 24h, and the mineralized aggregate body is obtained; S4. The polyimide solution is coated on the surface of the mineralized aggregate body with a coating thickness of 0.1 mm. After drying and forming a film for 2 minutes, a corrosion-resistant digital aggregate based on steric barrier is obtained.
[0035] Example 2 A corrosion-resistant digital aggregate based on steric barrier, other contents are the same as those in Example 1, except that the amount of sodium tetraborate used is 28 parts.
[0036] Example 3 A corrosion-resistant digital aggregate based on steric barrier, other contents are the same as those in Example 1, except that the amount of sodium tetraborate used is 35 parts.
[0037] Example 4 A corrosion-resistant digital aggregate based on steric barrier, other contents are the same as those of Example 1, except that the coating thickness of the polyimide solution is 0.2 mm.
[0038] Example 5 A corrosion-resistant digital aggregate based on three-dimensional barrier, other contents are the same as those of Example 1, except that the coating thickness of the polyimide solution is 0.4 mm.
[0039] Example 6 A corrosion-resistant digital aggregate based on steric barrier, other contents are the same as those in Example 1, except that the amount of chitosan used is 8 parts.
[0040] Example 7 A corrosion-resistant digital aggregate based on steric barrier, other contents are the same as those in Example 1, except that the amount of chitosan used is 10 parts.
[0041] Comparative Example 1 A corrosion-resistant digital aggregate based on three-dimensional barrier, the other contents are the same as those of Example 1, except that the first protective agent and the second protective agent are not included.
[0042] Test and Evaluation The corrosion-resistant digital aggregates prepared in each embodiment and comparative example were divided into two groups, one of which was directly used for compressive strength and signal transmission distance test in concrete; the other group was pre-immersed in 0.01mol / L dilute sulfuric acid solution for 24h, and the residual dilute sulfuric acid on the surface of the aggregate was treated after immersion, and then the digital aggregate was tested for compressive strength and signal transmission distance in concrete. The embedding depth of the digital aggregate in concrete is 2cm, and the signal transmission distance is read by a signal collector, and the working frequency of the signal collector is 433-950MHz ultra-high frequency. The compressive strength of the digital aggregate before and after immersion in corrosive media and its maximum reading distance in concrete are shown in Tables 1 and 2.
[0043] Table 1 Test results of compressive strength and maximum reading distance before immersion Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative Example 1 Compressive strength (MPa) 60.1 58.8 56.2 60.4 60.5 66.4 69.9 68.2 Reading distance in concrete (m) 2.4 2.4 2.3 2.5 2.4 2.7 3.1 2.6 Table 2 Test results of compressive strength and maximum reading distance after immersion Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative Example Compressive strength (MPa) 54.6 57.5 54.4 58.2 58.9 62.7 64.3 40.2 Reading distance in concrete (m) 2.0 2.2 2.2 2.3 2.2 2.2 2.5 1.2 Compared with Comparative Example 1, the compressive strength of the digital aggregate prepared in Examples 1-7 and the signal reading distance in concrete are not greatly affected by the dilute sulfuric acid solution. This is because the first protective agent has a high density and can physically block the intrusion of corrosive media in the external environment into the digital aggregate; at the same time, the second protective agent is added to the digital aggregate for use, and the hydrolysis-generated hydroxide can be combined with the corrosive media invading the digital aggregate to maintain the stability of the internal carbonization reaction products, thereby ensuring the strength of the digital aggregate and the stability of signal transmission.
[0044] It can be seen from Examples 1-3 that increasing the amount of the second protective agent used slightly decreases the compressive strength of the digital aggregate. This is because the second protective agent has no carbonization activity, and carbonates cannot be generated to fill the pores during the carbonation reaction, which leads to a decrease in the compressive strength of the digital aggregate. Comparing Example 1, Example 4 and Example 5, as the thickness of the first protective agent increases, the protective effect is enhanced, the invading corrosive substances are reduced, the digital aggregate is not corroded, and the compressive strength of the digital aggregate is not greatly affected. Comparing Example 1, Example 6 and Example 7, as the amount of reinforcing agent increases, the compressive strength of the digital aggregate increases. This is because the reinforcing agent can induce the production of more carbonate minerals to fill the pores in the carbon mineralization reaction, thereby increasing the compressive strength of the digital aggregate.
[0045] The present application uses two layers of protection measures to protect digital aggregates at the physical and chemical levels respectively, which cooperate with each other to block corrosive substances, maintain a relatively stable pH value in the internal environment, and protect the carbonization reaction products, thereby ensuring the stability of the digital aggregate strength signal transmission; when digital aggregates are used for identification management and quality traceability of concrete products, prefabricated components or cast-in-place structures, the problem of reduced digital aggregate signal transmission performance caused by external corrosive substances can be effectively avoided.
[0046] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A corrosion-resistant digital aggregate based on three-dimensional barrier, characterized in that: It includes a mineralized aggregate body and a first protective layer coated on the surface of the mineralized aggregate body; the aggregate body includes a radio frequency unit and a second protective layer coated on the radio frequency unit; the raw material of the first protective layer includes a first protective agent, and the first protective agent includes one or more of polyimide, fluorinated ethylene propylene copolymer, and soluble polytetrafluoroethylene; the raw material of the second protective layer includes a carbon mineralized material, a reinforcing agent, and a second protective agent, and the second protective agent includes one or more of sodium tetraborate, sodium silicate, and sodium aluminate.
2. The corrosion-resistant digital aggregate based on steric barrier according to claim 1, characterized in that: The mass ratio of the radio frequency unit, the carbon mineralization material, the first protective agent, the second protective agent and the reinforcing agent is 1:8-64:1-21:2-40:1-11.
3. The corrosion-resistant digital aggregate based on steric barrier according to claim 1, characterized in that: The carbon mineralization material includes one or more of tricalcium silicate, γ-type dicalcium silicate, β-type dicalcium silicate, monocalcium silicate, tricalcium disilicate, calcium hydroxide, magnesium hydroxide, calcium oxide, and magnesium oxide; the particle size of the carbon mineralization material is 75-150 μm.
4. The corrosion-resistant digital aggregate based on steric barrier according to claim 1, characterized in that: The enhancer includes one or more of chitosan, sodium alginate, polyethylene glycol and polyvinyl alcohol.
5. The corrosion-resistant digital aggregate based on steric barrier according to claim 1, characterized in that: The radio frequency unit includes a radio frequency chip and a radio frequency antenna connected to the radio frequency chip.
6. A method for preparing a corrosion-resistant digital aggregate based on steric barrier as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: S1. mixing the carbon mineralization material, the second protective agent, the reinforcing agent and water to obtain a mixture; S2. In a mold, the RF unit is embedded in the mixture, and pressed to obtain an aggregate body; S3. Under a carbon dioxide atmosphere, the aggregate body is mineralized to obtain a mineralized aggregate body; S4. Applying the first protective agent to the surface of the mineralized aggregate blank and drying it to form a film, the corrosion-resistant digital aggregate based on steric barrier is obtained.
7. The method for preparing corrosion-resistant digital aggregate based on steric barrier according to claim 6, characterized in that: In step S2, the pressing pressure is 10-60 MPa.
8. The method for preparing corrosion-resistant digital aggregate based on steric barrier according to claim 6, characterized in that: In step S3, the partial pressure of carbon dioxide is 0.1-0.3 MPa, the volume concentration of carbon dioxide is 20-99.9%, the mineralization temperature is 5-90° C., and the mineralization time is 12-48 hours.
9. The method for preparing corrosion-resistant digital aggregate based on steric barrier according to claim 6, characterized in that: In step S4, the coating thickness is 0.1-0.5 mm, and the film forming time is 1-3 min.
10. Application of the corrosion-resistant digital aggregate based on steric barrier obtained by the preparation method according to any one of claims 6 to 9 in the field of concrete components and / or cast-in-place structures.
Citation Information
Patent Citations
Easily-cleaned concrete product as well as preparation method and application thereof
CN110143790A
Anti-corrosion intelligent aggregate based on FRP coating
CN111157023A
Passive wireless temperature-sensitive digital aggregate as well as preparation method and application thereof
CN117263549A
Long-distance wireless identification digital aggregate as well as preparation method and application thereof
CN117447110A
Corrosion-resistant cementitious compositions
GB1207331A