High-performance composite admixture as well as preparation method and application thereof

Through the use of high-performance composite admixtures and the synergistic effect of solid waste resources such as coal gangue powder, iron tailings powder, lithium slag powder, etc., the problems of low concrete strength, durability and construction efficiency in the existing technology are solved, and the problem of low construction efficiency is achieved. Strength improvement, solidification acceleration and environmental protection requirements are met.

CN118754492APending Publication Date: 2024-10-11XIAMEN MEIYI ZHICHENG NEW MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410908376.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, when concrete uses admixtures, it is difficult to simultaneously improve strength, durability and construction efficiency, and the post-polymerization filling method of natural fibers reduces processing efficiency and construction efficiency.

Method used

The use of high-performance composite admixtures, including gangue powder, iron tailings powder, lithium slag powder, activators, surfactants and gap enhancers, improves the strength, durability and construction efficiency of concrete through synergistic effects, and achieves solidification. Comprehensive utilization of waste resources.

Benefits of technology

It has improved the strength and durability of concrete, accelerated the solidification process, shortened pouring and curing time, complied with environmental protection requirements, and improved the utilization rate of solid waste resources and construction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004932819620000071
    Figure BDA0004932819620000071
Patent Text Reader

Abstract

The invention relates to the technical field of concrete materials, in particular to a high-performance composite admixture and a preparation method and application thereof. The high-performance composite admixture is prepared from the following preparation raw materials in parts by mass: 190 to 210 parts of coal gangue powder, 90 to 100 parts of iron tailing powder, 180 to 200 parts of lithium slag powder, 5 to 6 parts of an exciting agent, 1 to 1.5 parts of a surfactant and 12 to 15 parts of a gap reinforcing agent. The high-performance composite admixture provided by the invention not only has excellent physical properties and crack resistance, but also can improve the production efficiency and realize comprehensive utilization of solid waste resources, meets the environmental protection requirements, and has wide application prospects and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of concrete materials, and in particular to a high-performance composite admixture and a preparation method and application thereof. Background Art

[0002] Gangue is the largest industrial solid waste in my country, with an accumulated volume of nearly 5 billion tons. The continuous generation and long-term open-air storage of gangue not only occupies a large amount of arable land and forest land, but also pollutes the air, surrounding soil and groundwater. Gangue has the properties of rock. The hard gangue can replace industrial aggregates to prepare concrete after processing. Gangue with high clay mineral content can be used as a cementitious material or admixture after heat treatment. Using gangue to prepare building materials can reduce the resource consumption and environmental damage caused by the mining of building material raw materials. At the same time, the large consumption of gangue can reduce the pollution of gangue to the environment, reduce the high emissions, high pollution and high energy consumption of the cement industry, and improve the comprehensive utilization rate of solid waste resources.

[0003] Iron tailings are the waste materials produced in the ore dressing process. my country produces more than 600 million tons of iron tailings every year, and the accumulated volume has reached 20 billion tons, accounting for more than 80% of industrial solid waste. However, the utilization rate of iron tailings in my country is only 7%, and the accumulation of a large amount of iron tailings will cause serious pollution to the environment. Therefore, it is very important to use appropriate methods to treat iron tailings. my country has a large storage capacity of spodumene concentrate, and the discharge of lithium slag has gradually increased with the development of industry. The composition of lithium slag is mainly amorphous SiO 2 and Al 2 O 3 It is mainly composed of volcanic ash and has certain volcanic ash activity, and can be used as a mineral admixture.

[0004] The role of admixtures is to improve the performance of concrete. In most cases, the 28-day compressive strength of concrete using admixtures should be correspondingly improved, and the fluidity should be close to the original concrete parameters. In order to fill concrete gaps and improve adhesion, the prior art also adds natural fibers (particles) to improve the adhesion of the concrete itself and the structural strength of the concrete after molding. However, natural fibers themselves can only significantly improve their performance after polymerization. The prior art adopts the method of first polymerization and then filling in the admixture, which reduces the processing efficiency of the admixture and the construction efficiency of the concrete. Summary of the invention

[0005] The purpose of this application is to address the deficiencies of current technology and provide a high-performance composite admixture and its preparation method and application. When the high-performance composite admixture provided by this application replaces cement to prepare concrete, it can not only ensure the strength and durability of the concrete, but also accelerate the solidification of the concrete, shorten the pouring and curing time, and at the same time realize large-scale resource comprehensive utilization of solid waste, which meets environmental protection requirements.

[0006] In the first aspect, the present application provides a high-performance composite admixture, which adopts the following technical solution: A high-performance composite admixture comprises the following raw materials by weight: 190-210 parts of coal gangue powder, 90-100 parts of iron tailings powder, 180-200 parts of lithium slag powder, 5-6 parts of activator, 1-1.5 parts of surfactant and 12-15 parts of gap enhancer.

[0007] By adopting the above technical solution, coal gangue powder: coal gangue powder mainly provides SiO 2 and Al 2 O 3 Iron tailings powder: Iron tailings powder contains a large amount of active SiO 2 and Al 2 O 3 , can react with Ca(OH) 2 The reaction generates hydration products such as hydrated calcium silicate, which improves the strength and durability of concrete. Lithium slag powder: Amorphous SiO 2 and Al 2 O 3 It has volcanic ash activity and can be used as a mineral admixture to help improve the performance of concrete. Activator: The activator can accelerate the solidification process of concrete, shorten the pouring and curing time, and improve construction efficiency. Surfactant: The use of surfactants can reduce the dissolution of heavy metal ions in admixtures, meet green environmental protection requirements, and improve the performance of concrete. Gap enhancer: The gap enhancer is used to fill cement gaps and improve adhesion, which helps to improve the strength and durability of concrete. Combining the effects and synergistic effects of the above components, high-performance composite admixtures can effectively improve the strength, durability and construction efficiency of concrete, while meeting environmental protection requirements and realizing the comprehensive utilization of solid waste resources.

[0008] Preferably, the mass ratio of the coal gangue powder, the iron tailings powder and the lithium slag powder is 2:1:2.

[0009] By adopting the above technical solution, coal gangue powder: as one of the main ingredients, coal gangue powder provides a high content of SiO 2 and Al 2 O 3 , which helps to increase the strength and durability of concrete. At the same time, the Fe and S elements in it can also have a certain impact on the performance of concrete, comprehensively improving the overall performance of concrete. Iron tailings powder: The active SiO in iron tailings powder 2 and Al 2 O 3 Can react with Ca(OH) 2The reaction generates hydration products such as hydrated calcium silicate, thereby improving the strength and durability of concrete. The role of iron tailings powder here is to promote the hydration reaction. Lithium slag powder: The amorphous SiO 2 and Al 2 O 3 It has volcanic ash activity and can be used as a mineral admixture to promote the performance of concrete to a certain extent, further improving the overall performance of concrete. Through the reasonable proportion of the above three raw materials, they work together to improve the strength and durability of concrete while accelerating the solidification process of concrete, shortening the construction period, and achieving comprehensive resource utilization and environmental protection requirements. Integrating the characteristics and functions of various components, the synergistic results will make a positive contribution to the goal of preparing high-performance composite admixtures.

[0010] Preferably, the thermal activation method of the coal gangue powder is: using tap water to wash the carbon on the surface of the coal gangue, and then putting it into an oven for drying. After drying, mechanical crushing is used to grind the crushed coal gangue to an average particle size of 0.075 mm, and then roasting at 500-550°C for 2-3h to obtain coal gangue powder.

[0011] By adopting the above technical solution, the activity of the coal gangue can be improved by thermally activating the coal gangue by a roasting method, thereby accelerating the solidification of concrete.

[0012] Preferably, the activator is prepared by mixing calcium hydroxide and sodium hydroxide in a mass ratio of 7:1-2.

[0013] By adopting the above technical solution, the activator is prepared by mixing calcium hydroxide and sodium hydroxide and used in a certain mass ratio. The activator plays a role in accelerating the hydration reaction in concrete, thereby promoting the early strength development of concrete and shortening the effect of setting time. Calcium hydroxide can increase the alkalinity in concrete, promote the hydration reaction rate of minerals in cement, and improve the early strength of concrete. Sodium hydroxide also has a similar function and can react with silicates in cement to form gelling substances and accelerate the solidification of concrete. Through the synergistic effect of calcium hydroxide and sodium hydroxide, the activator can promote the hydration reaction in cement faster, accelerate the generation of silicates and calcium compounds, and form more hydration products, thereby improving the strength and early hardening speed of concrete. This synergistic effect helps to shorten the setting time of concrete and improve the overall engineering construction efficiency.

[0014] Preferably, the surfactant is prepared by mixing sodium lauryl sulfate and alkylphenol polyoxyethyl ether in a mass ratio of 5:1-2.

[0015] By adopting the above technical scheme, the role of surfactants in high-performance composite admixtures has two main aspects: on the one hand, it reduces the dissolution of heavy metal ions in the admixture, thereby improving the environmental performance of concrete; on the other hand, it can enhance the adhesion between the admixture and cement, and improve the overall strength and durability of concrete. The synergistic effect between the two surfactants, sodium dodecyl sulfate and alkylphenol polyoxyethyl ether, can improve the impermeability and durability of concrete. Sodium dodecyl sulfate has good permeability and permeability regulation, while alkylphenol polyoxyethyl ether has the effects of humidification, dispersion and foam stabilization. The combination of the two can better improve the performance and process performance of concrete. Therefore, the synergistic effect of these two surfactants in high-performance composite admixtures can make concrete more uniform, dense and durable.

[0016] Preferably, the gap enhancer is prepared by mixing carbon fiber and a modifier in a mass ratio of 100:2-4, and the length of the carbon fiber is 3-5 mm.

[0017] By adopting the above technical scheme, the role of the gap enhancer in the high-performance composite admixture is to fill the cement gap and improve the bonding force, thereby improving the overall strength and durability of the concrete. When carbon fiber is used as a gap enhancer in concrete, the carbon fiber can effectively fill the tiny cracks inside the concrete and improve the tensile strength and impact resistance of the concrete. Carbon fiber can also improve the crack resistance of concrete, reduce the shrinkage cracks of concrete, and extend the service life of concrete. The synergistic effect of carbon fiber and modifier in the gap enhancer is mainly to improve the bonding force and adhesion between carbon fiber and concrete, while the modifier can improve the properties of the carbon fiber surface, increase its dispersibility and compatibility, and make it better interact with concrete. The modifier can also further improve the interaction between concrete and the gap enhancer, thereby enhancing the overall performance of concrete. Through the synergistic effect of carbon fiber and modifier, the tensile strength, impact resistance and durability of concrete can be effectively improved, and the preparation of high-performance concrete can be achieved.

[0018] Preferably, the preparation method of the modifier comprises the following steps: S71, according to the mass parts, 10 parts of polyvinyl alcohol, 10-12 parts of polyvinyl pyrrolidone and 20-25 parts of alkylphenol polyoxyethyl ether were mixed evenly, and then 300 parts of water were added, stirred to dissolve, dried, crushed, and sieved through 100 mesh to obtain a mixture A; S72. Mix 10-12 parts of lime and 2-3 parts of calcium hydroxide in parts by mass, add them to mixed material A, mix well, and obtain a modifier.

[0019] By adopting the above technical scheme, the role of the modifier in the high-performance composite admixture is to enhance the mechanical properties, durability and crack resistance of the concrete by improving the structural stability and adhesion inside the concrete. The modifier can improve the compatibility and adhesion between the admixture and the cement matrix, enhance its dispersibility and uniformity in the concrete, thereby improving the durability and overall performance of the concrete. The modifier is prepared from raw materials such as polyvinyl alcohol, polyvinyl pyrrolidone, alkylphenol polyoxyethyl ether, lime and calcium hydroxide. Polyvinyl alcohol and polyvinyl pyrrolidone have the function of thickening and improving the dispersibility of concrete, and alkylphenol polyoxyethyl ether can improve the adhesion and dispersibility of the modifier. The role of lime and calcium hydroxide in the modifier is to further enhance the function of the modifier by reacting with other components, and can promote its interaction with the cement matrix in the concrete to improve the overall performance. The synergistic effect of the modifier is to achieve the optimal ratio and effect of various additives in the concrete through the interaction between the components. Polyvinyl alcohol, polyvinyl pyrrolidone and alkylphenol polyoxyethyl ether act on the modifier together, and synergistically play the effect of improving the performance of concrete. The addition of lime and calcium hydroxide can further improve the chemical activity and functionality of the modifier, thereby strengthening the interaction between the modifier and concrete, and achieving the purpose of improving the performance of concrete. Through the synergistic effect between the modifier components, the overall performance and environmental performance of high-performance composite admixtures can be effectively improved.

[0020] In the second aspect, the present application provides a method for preparing a high-performance composite admixture, adopting the following technical scheme: As a general technical concept, the present application also provides a method for preparing the above-mentioned high-performance composite admixture, comprising the following steps: first, according to the mass fractions, mix the coal gangue powder, iron tailings powder and lithium slag powder evenly, then add the activator, surfactant and gap enhancer in sequence and mix evenly to obtain a high-performance composite admixture.

[0021] In a third aspect, the present application provides an application of a high-performance composite admixture, using the following technical solution: As a general technical concept, the present application also provides an application of the above-mentioned high-performance composite admixture, where the high-performance composite admixture replaces 15-25wt% of the cement required in concrete.

[0022] In summary, the beneficial technical effects of this application are: 1. Ensure the strength and durability of concrete: By replacing cement with high-performance composite admixtures, the strength and durability of concrete can be guaranteed, and the concrete can have better mechanical properties and crack resistance.

[0023] 2. Accelerate the solidification of concrete and shorten the pouring and curing time: Adding activators can accelerate the solidification process of concrete, thereby shortening the pouring and curing time and improving production efficiency.

[0024] 3. Realize large-scale comprehensive utilization of solid waste resources: The raw materials in high-performance composite admixtures include solid waste resources such as coal gangue powder, iron tailings powder and lithium slag powder. By utilizing these solid waste resources to prepare high-performance composite admixtures, large-scale comprehensive utilization of solid waste resources is achieved, achieving the goals of environmental protection and sustainable development.

[0025] 4. Reduce the dissolution amount of heavy metal ions in admixtures: The use of surfactants can effectively reduce the dissolution amount of heavy metal ions in admixtures, improve the environmental performance of high-performance composite admixtures, and meet the requirements of green production. DETAILED DESCRIPTION

[0026] The embodiments of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially. Coal gangue is taken from a gangue mountain in Bijie, Guizhou, and iron tailings are taken from Waitou Mountain, Liaoning; lithium slag powder is taken from Qinzhou City, Guangxi.

[0027] Preparation Example 1 Coal Gangue Powder The thermal activation method of coal gangue powder is as follows: the carbon on the surface of the coal gangue is washed with tap water, and then placed in an oven for drying. After drying, the crushed coal gangue is ground to an average particle size of 0.075 mm by mechanical crushing, and then calcined at 530°C for 2.5 hours to obtain coal gangue powder.

[0028] The coal gangue powder prepared above is applied to each embodiment.

[0029] Preparation Example 2 Preparation of Modifier The preparation method of the modifier comprises the following steps: S71, according to the mass fractions, 10kg of polyvinyl alcohol, 11kg of polyvinyl pyrrolidone and 22kg of alkylphenol polyoxyethyl ether were mixed uniformly, and then 300kg of water was added, stirred to dissolve, dried, crushed, and sieved through 100 mesh to obtain a mixture A; S72. According to the mass fractions, 12 kg of lime and 2.5 kg of calcium hydroxide are mixed evenly, and then added into the mixture A, and mixed evenly to obtain a modifier.

[0030] The modifier prepared above was applied to each example.

[0031] Example 1 A high-performance composite admixture, comprising the following raw materials by weight: 190 kg of coal gangue powder, 100 kg of iron tailings powder, 180 kg of lithium slag powder, 5 kg of activator, 1 kg of surfactant, and 12 kg of gap enhancer, wherein the activator is prepared by mixing calcium hydroxide and sodium hydroxide in a weight ratio of 7:1, the surfactant is prepared by mixing sodium dodecyl sulfate and alkylphenol polyoxyethyl ether in a weight ratio of 5:1, the gap enhancer is prepared by mixing carbon fiber and a modifier in a weight ratio of 100:2, and the length of the carbon fiber is 3-5 mm; The preparation method of the above-mentioned high-performance composite admixture is to first mix coal gangue powder, iron tailings powder and lithium slag powder evenly according to the mass proportions, and then add an activator, a surfactant and a gap enhancer in sequence and mix them evenly to obtain a high-performance composite admixture.

[0032] Example 2 A high-performance composite admixture, comprising the following raw materials by weight: 210 kg of coal gangue powder, 90 kg of iron tailings powder, 200 kg of lithium slag powder, 6 kg of activator, 1.5 kg of surfactant, and 15 kg of gap enhancer, wherein the activator is prepared by mixing calcium hydroxide and sodium hydroxide in a weight ratio of 7:2, the surfactant is prepared by mixing sodium dodecyl sulfate and alkylphenol polyoxyethyl ether in a weight ratio of 5:2, the gap enhancer is prepared by mixing carbon fiber and a modifier in a weight ratio of 100:4, and the length of the carbon fiber is 3-5 mm; The preparation method of the above-mentioned high-performance composite admixture is to first mix coal gangue powder, iron tailings powder and lithium slag powder evenly according to the mass proportions, and then add an activator, a surfactant and a gap enhancer in sequence and mix them evenly to obtain a high-performance composite admixture.

[0033] Example 3 A high-performance composite admixture, comprising the following raw materials by weight: 200 kg of coal gangue powder, 92 kg of iron tailings powder, 190 kg of lithium slag powder, 5.5 kg of activator, 1.3 kg of surfactant, and 14 kg of gap enhancer, wherein the activator is prepared by mixing calcium hydroxide and sodium hydroxide in a weight ratio of 7:1.5, the surfactant is prepared by mixing sodium dodecyl sulfate and alkylphenol polyoxyethyl ether in a weight ratio of 5:1.5, the gap enhancer is prepared by mixing carbon fiber and a modifier in a weight ratio of 100:3, and the length of the carbon fiber is 3-5 mm; The preparation method of the above-mentioned high-performance composite admixture is to first mix coal gangue powder, iron tailings powder and lithium slag powder evenly according to the mass proportions, and then add an activator, a surfactant and a gap enhancer in sequence and mix them evenly to obtain a high-performance composite admixture.

[0034] Example 4 The same as Example 3, except that there are 192.8 kg of coal gangue powder, 96.4 kg of iron tailings powder, and 192.8 kg of lithium slag powder.

[0035] Comparative Example 1 The same as Example 4, except that the activator is calcium hydroxide.

[0036] Comparative Example 2 The same as Example 4, except that the activator is sodium hydroxide.

[0037] Comparative Example 3 The same as Example 4, except that the gap enhancer is carbon fiber, and the length of the carbon fiber is 3-5 mm.

[0038] Comparative Example 4 The same as Example 4, except that the surfactant is sodium dodecyl sulfate.

[0039] Comparative Example 5 The same as Example 4, except that the surfactant is alkylphenol polyoxyethyl ether.

[0040] Performance Testing The high-performance composite admixtures prepared in Examples 1 to 4 and Comparative Examples 1 to 5 were used to make concrete specimens. The concrete specimens were cubes with a side length of 100 mm. The surface was sealed with a polyethylene film and cured at room temperature for 24 hours before demolding. The specimens were moved to a standard curing box and cured to the corresponding age. Performance tests were performed. The test results are shown in Table 1. The concrete consisted of the following components by weight: 260 kg of P.O42.5 cement, 80 kg of fly ash, 1000 kg of 5-16 mm continuous graded crushed stone, 600 kg of river sand with an average particle size of 0.3 mm, 166 kg of water, 4.5 kg of polycarboxylic acid water reducer and 60 kg of high-performance composite admixture. In the experiment, the control group: concrete consisted of the following components by weight: 300 kg of P.O42.5 cement, 80 kg of fly ash, 1000 kg of 5-16 mm continuous graded crushed stone, 600 kg of river sand with an average particle size of 0.3 mm, 166 kg of water and 4.5 kg of polycarboxylate water reducer.

[0041] The compressive strength is tested according to the national standard GB / T17671-2021 after the specimen is cured for 28 days; Activity index: tested according to GB / T12957-2005 "Test method for activity of industrial waste residue used in cement admixtures"; heavy metal dissolution: tested according to the test method in Appendix A of "Identification standard for hazardous waste - leaching toxicity identification" GB5085.3-2007.

[0042] Table 1 Performance test In the table, — indicates that no test was performed.

[0043] Analyzing the data in Table 1, we can see that: 1) When the high-performance composite admixtures prepared in Examples 1 to 4 replace 20 wt% of cement, the obtained concrete has higher compressive strength, activity index and lower heavy metal dissolution, indicating that when the high-performance composite admixtures provided in this application are used to replace cement to prepare concrete, not only can the strength and durability of the concrete be guaranteed, but also the solidification of the concrete can be accelerated, the pouring and curing time can be shortened, and at the same time, large-scale resource comprehensive utilization of solid waste can be realized, which meets environmental protection requirements.

[0044] 2) The performance comparison analysis of the high-performance composite admixtures prepared in combination with Example 4 and Example 1-Example 3 to replace cement to prepare concrete shows that when the mass ratio of the coal gangue powder, the iron tailings powder and the lithium slag powder is 2:1:2. Through the reasonable proportion of the above three raw materials, they work together to improve the strength and durability of concrete, accelerate the solidification process of concrete, shorten the construction period, and achieve comprehensive resource utilization and environmental protection requirements.

[0045] 3) The performance comparison analysis of the concrete prepared by replacing cement with the high-performance composite admixture prepared in combination with Example 4 and Comparative Examples 1-2 shows that the activator is prepared by mixing calcium hydroxide and sodium hydroxide in a mass fraction ratio of 7:1.5. The activator plays a role in accelerating the hydration reaction in concrete, thereby promoting the early strength development of concrete and shortening the effect of setting time. Calcium hydroxide can increase the alkalinity in concrete, promote the hydration reaction rate of minerals in cement, and improve the early strength of concrete. Sodium hydroxide also has a similar function, which can react with silicates in cement to form gelling substances and accelerate the solidification of concrete. Through the synergistic effect of calcium hydroxide and sodium hydroxide, the activator can promote the hydration reaction in cement faster, accelerate the generation of silicates and calcium compounds, and form more hydration products, thereby improving the strength and early hardening speed of concrete. This synergistic effect helps to shorten the setting time of concrete and improve the overall engineering construction efficiency.

[0046] 4) The performance comparison analysis of the concrete prepared by replacing cement with the high-performance composite admixture prepared in combination with Example 4 and Comparative Example 3 shows that the gap enhancer is prepared by mixing carbon fiber and modifier in a mass ratio of 100:3. The synergistic effect of carbon fiber and modifier in the gap enhancer is mainly to improve the bonding force and adhesion between carbon fiber and concrete. At the same time, the modifier can improve the properties of the carbon fiber surface, increase its dispersibility and compatibility, and make it better interact with concrete. The modifier can also further improve the interaction between concrete and the gap enhancer, thereby enhancing the overall performance of concrete. Through the synergistic effect of carbon fiber and modifier, the tensile strength and durability of concrete can be effectively improved.

[0047] 5) The performance comparison analysis of the concrete prepared by replacing cement with the high-performance composite admixtures prepared in combination with Example 4 and Comparative Examples 4-5 shows that the surfactant is prepared by mixing sodium lauryl sulfate and alkylphenol polyoxyethyl ether in a mass ratio of 5:1.5. The dissolution amount of heavy metal ions in concrete is reduced, thereby improving the environmental performance of concrete; the bonding force between the admixture and cement can be enhanced, and the overall strength and durability of concrete can be improved. The synergistic effect between the two surfactants, sodium lauryl sulfate and alkylphenol polyoxyethyl ether, can improve the impermeability and durability of concrete. The combination of the two can better improve the performance of concrete. Therefore, the synergistic effect of the two surfactants in the high-performance composite admixture can make the concrete more uniform, dense and durable.

[0048] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A high performance composite admixture, characterized in that: The preparation raw materials include the following by weight: 190-210 parts of coal gangue powder, 90-100 parts of iron tailings powder, 180-200 parts of lithium slag powder, 5-6 parts of activator, 1-1.5 parts of surfactant and 12-15 parts of gap enhancer.

2. A high performance composite admixture according to claim 1, characterized in that: The mass ratio of the coal gangue powder, the iron tailings powder and the lithium slag powder is 2:1:

2.

3. A high performance composite admixture according to claim 1, characterized in that: The thermal activation method of the coal gangue powder is: using tap water to wash the carbon on the surface of the coal gangue, then putting it into an oven for drying, after drying, using mechanical crushing to grind the crushed coal gangue to an average particle size of 0.075mm, and then roasting it at 500-550℃ for 2-3h to obtain the coal gangue powder.

4. A high performance composite admixture according to claim 1, characterized in that: The activator is prepared by mixing calcium hydroxide and sodium hydroxide in a mass ratio of 7:1-2.

5. The high performance composite admixture according to claim 1, characterized in that: The surfactant is prepared by mixing sodium lauryl sulfate and alkylphenol polyoxyethyl ether in a mass ratio of 5:1-2.

6. A high performance composite admixture according to claim 1, characterized in that: The gap enhancer is prepared by mixing carbon fiber and a modifier in a mass ratio of 100:2-4, and the length of the carbon fiber is 3-5 mm.

7. A high performance composite admixture according to claim 6, characterized in that: The preparation method of the modifier comprises the following steps: S71, according to the mass parts, 10 parts of polyvinyl alcohol, 10-12 parts of polyvinyl pyrrolidone and 20-25 parts of alkylphenol polyoxyethyl ether were mixed evenly, and then 300 parts of water were added, stirred to dissolve, dried, crushed, and sieved through 100 mesh to obtain a mixture A; S72. Mix 10-12 parts of lime and 2-3 parts of calcium hydroxide in parts by mass, add them to mixed material A, mix well, and obtain a modifier.

8. A method for preparing a high-performance composite admixture according to any one of claims 1 to 7, characterized in that: The following steps are involved: According to the mass proportions, the coal gangue powder, iron tailings powder and lithium slag powder are first mixed evenly, and then the activator, surfactant and gap enhancer are added in sequence and mixed evenly to obtain a high-performance composite admixture.

9. An application of a high-performance composite admixture according to any one of claims 1 to 7, characterized in that: The high-performance composite admixture replaces 15-25 wt% of the cement required in concrete.

Citation Information

Patent Citations

  • Method for preparing high-performance concrete by using gangue as main raw material

    CN105622013A

  • Multiwall carbon nanotube cement-based composite material and preparation method thereof

    CN108358521A

  • Iron tailing activation method and multi-solid-waste iron tailing concrete

    CN113149500A

  • Solid waste-based composite lithium slag ultra-fine admixture as well as preparation method and application thereof

    CN114315184A

  • Lead-zinc tailing concrete composite admixture and preparation method thereof

    CN115259725A