Low-carbon electric furnace slag-red mud-based cement printing ink material as well as preparation method and application thereof
By using low-carbon electric furnace slag-red mud-based cement ink materials in 3D printing ink materials, the hydration activity of electric furnace slag is stimulated, which solves the problems of slow hydration activity and high carbon dioxide emissions of materials in traditional technology, and realizes the hydration of materials. Early strengthening effect and improved environmental protection.
Patent Information
- Application Number
- CN202410801414.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-11
AI Technical Summary
The traditional construction industry has problems with waste of building materials and high carbon dioxide emissions. Moreover, the hydration activity of electric furnace slag in 3D printing ink materials is slow and cannot meet the rapid condensation requirements, limiting its utilization.
Low-carbon electric furnace slag-red mud-based cement ink material is used. Electric furnace slag and red mud are mixed and processed by ultra-fine tire vertical mill to form 500-700 mesh ultra-fine powder, which is combined with ordinary cement, sand, double-fast cement, and silicon. Ash, water-reducing agent and expansion agent control the performance factor and carbon reduction factor within a specific range to form a CaO-SiO2-Al2O3 system, which stimulates the hydration activity of electric furnace slag and replaces the use of some double-fast cement and ordinary cement.
It achieves the early strength effect of electric furnace slag, reduces the cost of construction 3D printing ink materials, reduces carbon dioxide emissions, improves the fluidity and interlayer bonding strength of materials, and improves the strength and environmental protection of 3D printed components.
Smart Images

Figure BDA0004903486000000141
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of building 3D printing and solid waste resource utilization, and specifically relates to a low-carbon electric furnace slag-red mud-based cement ink material, a preparation method and an application thereof. Background Art
[0002] With the development of society, industrial automation is also developing rapidly, but the automation level of traditional construction industry needs to be improved. The traditional construction industry has always had problems such as waste of building materials, construction methods are limited by the shape and production of templates, and concrete construction requires a lot of manual participation. These problems restrict the development of traditional construction industry. Architectural 3D printing technology can control the use of materials as needed, thereby effectively reducing waste, and architectural 3D printing technology can also print complex building structures as needed to increase the freedom of architectural design. Architectural 3D printing technology can also realize automated production, thereby reducing labor costs and saving time.
[0003] As a traditional building material, cement is in great demand every year. At present, cement is mainly made by calcining limestone, clay and iron ore. A large amount of carbon dioxide will be produced in the process of producing cement. For every ton of cement produced, nearly one ton of carbon dioxide will be produced. Carbon dioxide, as the main gas causing the greenhouse effect, has a great impact on the environment. Therefore, using solid waste instead of cement is one of the development directions of the construction industry.
[0004] Since the ink material used in architectural 3D printing technology needs to have the characteristics of rapid solidification, double-fast cement is generally used. However, the large-scale use of double-fast cement does not meet the development needs of green buildings. How to ensure the performance characteristics of ink materials and avoid the use of double-fast cement as much as possible has become a key research direction in this field.
[0005] Electric furnace slag is a solid waste discharged during the process of smelting metals in electric furnaces. As an industrial power, my country also discharges a large amount of electric furnace slag every year. Electric furnace slag contains dicalcium silicate and tricalcium silicate and other components with hydration activity. Reasonable use can produce early strength effect on cementitious materials. Studies have found that because electric furnace slag is difficult to grind and has slow hydration activity in the early stage, the utilization rate of electric furnace slag is very low. At the same time, due to the unique characteristics of the ink material of 3D printing technology, its electric furnace slag as a cementitious material cannot meet the ink material parameter requirements of 3D printing technology. Summary of the invention
[0006] In order to solve the above technical problems, the inventors have obtained the technical solution of the present invention through practice and summary. The present invention adopts the following technical solution:
[0007] A low-carbon electric furnace slag-red mud-based cement ink material, characterized in that the ink material comprises the following components in parts by weight: 34 to 44 parts of ordinary cement, 20 to 30 parts of electric furnace slag-red mud mixed slag, 100 to 110 parts of sand, 4 to 10 parts of double-fast cement, 4 to 10 parts of silica fume, 0.6 to 1.0 parts of water reducer, 6 to 12 parts of expansion agent and 20 to 30 parts of water.
[0008] In the ink material, the mass ratio of the mixture of 500-700 mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 500-700 mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is (2-4):1.
[0009] In the ink material, the red mud is red mud ultrafine powder that has been ground to 500-700 mesh by ultrafine tire vertical grinding, and the chemical composition and mass percentage are: SiO 2 11.26%~12.21%, CaO 19.76%~21.30%, MgO0.85%~1.46%, A1 2 O 3 31.29%~33.60%, Fe 2 O 3 6.38%~10.02%, K 2 O 0.36%~0.62%, Na 2 O2.35%~4.20%, the remainder is impurities;
[0010] The electric furnace slag is an electric furnace slag ultrafine powder obtained by ultrafine tire vertical grinding to 500-700 meshes, and its chemical composition and mass percentage are as follows: CaO 34.13-38.34%, Fe 2 O 3 34.42%~43.01%, SiO 2 9.42%~12.57%, MgO2.11%~4.12%, MnO3.01%~4.42%, P 2 O 5 0.64%~1.43%,Al 2 O 3 4.01%~5.91%, the remainder is impurities;
[0011] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud+electric furnace slag), 0.714≤PF≤0.768;
[0012] Carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO2 +A1 2 O 3 ), 0.383≤CRF≤0.436;
[0013] in:
[0014] M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content of
[0015] M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 Total content of
[0016] M (red mud + electric furnace slag) is the total content of the mixed slag.
[0017] In the ink material, the sand includes quartz sand and / or machine-made sand, and the particle size is 0.075 to 0.5 mm;
[0018] The ordinary cement is ordinary Portland cement with a strength of 42.5;
[0019] The silica fume is microsilica powder SiO 2 The content is 92% to 98%;
[0020] The water reducer is a polycarboxylate water reducer in the form of powder;
[0021] The double-fast cement is sulphoaluminate cement;
[0022] The expansion agent is a UEA concrete expansion agent, and the material form is powder;
[0023] The water is tap water.
[0024] A method for preparing a low-carbon electric furnace slag-red mud-based cement ink material comprises the following steps:
[0025] 1) Mix ordinary cement, double-fast cement, silica fume, sand, expansion agent and water reducing agent to obtain a basic mixture:
[0026] 2) fully mixing the electric furnace slag and the red mud and adding them to the base mixture in batches to obtain a mixture precursor;
[0027] 3) adding water in batches to the mixture precursor for mixing and stirring to obtain a low-carbon electric furnace slag-red mud-based cement ink material.
[0028] In the method for preparing the ink material, the mixing and stirring speed in step 1) is 100 to 200 rpm, and the time is 120 to 300 s.
[0029] In the method for preparing the ink material, in step 2), the stirring speed when mixing the electric furnace slag and the red mud is 100 to 150 rpm, and the stirring time is 120 to 180 s;
[0030] The stirring speed for each addition is 100-200 rpm, and the stirring time after each addition is 180-420 s.
[0031] In the method for preparing the ink material, in step 3), 50% of water is first added to the mixture precursor for mixing and stirring, and the stirring speed is 100 to 200 rpm for 60 to 180 seconds.
[0032] In the method for preparing the ink material, in step 3), 50% of water is added to the mixture precursor for mixing and stirring at a stirring speed of 300 to 500 rpm for 300 to 600 seconds.
[0033] An application of a low-carbon electric furnace slag-red mud-based cement ink material, wherein the ink material is applied to 3D printing building materials and steam curing of printed components.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1) In terms of red mud application, because red mud has a high alkalinity of about 12.1 to 13.0, its high alkalinity greatly increases the difficulty of red mud application. If red mud is used directly without treatment, due to its strong alkalinity, it will cause alkali-aggregate reaction, which will destroy the concrete structure and affect its strength and durability. At the same time, it will also cause frosting, and white substances will appear on the surface of the concrete, affecting the appearance and performance of the concrete. The current process for dealkalization of red mud mainly uses acid washing to neutralize its strong alkalinity. However, in the process of dealkalization in this way, there are problems such as large acid consumption, high equipment corrosion resistance requirements, large equipment loss, and secondary pollution. Therefore, it cannot be fully promoted as a reliable way to apply red mud dealkalization.
[0036] The inventors have found through research that by mixing electric furnace slag and red mud for use, the early hydration activity of the electric furnace slag can be stimulated in the soluble alkaline environment produced by the red mud, thereby producing an early strength effect and solving the problem of slow stimulation of the hydration activity of the electric furnace slag. This effect can replace the use of part of the double-fast cement.
[0037] The introduction of electric furnace slag into building materials can effectively solve the negative impact of alkalinity caused by the direct use of red mud. At the same time, it can stimulate the hydration activity of electric furnace slag, achieve early strength effect, and thus replace the use of part of double-fast cement.
[0038] The cementitious material of the electric furnace slag and red mud compound used in the present invention is CaO-SiO 2 -Al 2 O 3 system, and the Al in the system 2 O 3 It has a high content and the characteristics of aluminosilicate, and can replace part of ordinary cement.
[0039] The present invention adopts red mud and electric furnace slag as gelling materials in 3D printing ink materials, thereby reducing the use of ordinary cement. The strong alkalinity of red mud and the precise amount of electric furnace slag can stimulate the hydration activity of the electric furnace slag, achieve early strength effect, and can replace part of the double-fast cement. This reduces the cost of building 3D printing ink materials, achieves carbon reduction in the building 3D printing industry, and responds to the national dual-carbon policy.
[0040] 2) The inventors have found through a large number of experimental studies that when PF is less than 0.714, the strength of the mixed slag is insufficient, affecting the performance of concrete; when PF is greater than 0.768, the chemical composition of the cement is unbalanced, causing problems such as cracks and falling off of the cement during long-term use, and the durability is reduced.
[0041] The inventors have found through a large number of experimental studies that when CRF < 0.383, it is not conducive to the formation of CaO-SiO mixed slag. 2 -Al 2 O 3 system, which is not conducive to the mixed slag playing the role of double-fast cement material; when CRF>0.436, it will cause poor thermal stability of the material and affect the later strength of the cement-based material, which is not conducive to the mixed slag playing the role of ordinary cement material.
[0042] Therefore, the present invention strictly controls the chemical composition and mass percentage of the mixed slag, and according to the performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), 0.714≤PF≤0.768; carbon reduction factor CRF=M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), 0.383≤CRF≤0.436, which is used to solve the problem that the traditional method of directly using electric furnace slag as a cementitious material cannot meet the ink material parameter requirements of 3D printing technology.
[0043] 3) The electric furnace slag used in the present invention is a waste product of scrap steel smelting. The free calcium oxide content in the electric furnace slag is very low, so it has good stability. The electric furnace slag and red mud are processed by ultra-fine tire vertical mill, and the particle size is small (500-700 mesh), which can be better dispersed in the cement material. And after ultra-fine wheel vertical mill, the smaller particle size is conducive to improving the fluidity and interlayer bonding strength of the mortar, ensuring smooth discharge port during 3D printing.
[0044] 4) The water reducer, expander and other materials (except water) used in the present invention are in powder form. Laboratory research has found that when the traditional liquid cement ink material is mixed with the water reducer and expander parts (liquid), the material cannot be homogenized. Due to the intermolecular force, the material (water reducer, expander and other materials) will be wrapped by the cementitious material powder to form tiny monomers, which is not conducive to the full mixing of the materials, thus affecting the strength performance of the components printed later. Therefore, compared with the traditional cement ink material containing liquid components, the powdered material used in this application is conducive to solving the impact of uneven distribution between materials on material performance, so that the strength performance of the components can be improved by one to two percentage points. At the same time, the powdered material form is convenient for transportation, production and processing, and on-site compounding.
[0045] 5) The present invention strictly compounds electric furnace slag and red mud, partially replaces the amount of double-fast cement, and combines it with 3D printing intelligent building technology to prepare an electric furnace slag-red mud-based cement ink material that meets the requirements of 3D printing and has low carbon properties. It makes full use of smelting solid waste resources and the on-site construction advantages of 3D printing, which is not only conducive to solving the problem that traditional construction industry requires a large amount of manual participation, but also helps to solve the problem of resource recycling of electric furnace slag and red mud, and has high environmental protection and economic benefits.
[0046] 6) The low-carbon electric furnace slag-red mud-based cement ink material proposed in the present invention has a lower consistency than ordinary cement ink materials, which is more conducive to the smoothness of the discharge port of the 3D printing instrument. Its 3D cube compressive strength is increased by 20% to 40% compared with ordinary cement ink materials, and its later strength changes little compared with ordinary cement ink materials. DETAILED DESCRIPTION
[0047] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0048] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.
[0049] Embodiment 1:
[0050] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0051] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0052] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 3:1.
[0053] The chemical composition and mass percentage of the red mud are: SiO 2 11.38%, CaO20.21%, MgO1.12%, A1 2 O 3 32.24%, Fe 2 O 3 6.98%, K 2 O 0.47%, Na 2 O 3.75%, the remainder is impurities.
[0054] The chemical composition and mass percentage of the electric furnace slag are: CaO 36.27%, Fe 2 O 3 39.44%, SiO 2 10.89%, MgO 3.11%, MnO 3.20%, P 2 O 5 1.03%, A l 2 O 3 4.28%, the remainder is impurities.
[0055] Performance factor PF=M(CaO+SiO 2 +A12 O 3 ) / M(red mud + electric furnace slag), PF = 0.7437 (rounded off); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.4158 (rounded);
[0056] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0057] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0058] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0059] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0060] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0061] Embodiment 2:
[0062] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0063] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0064] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 2:1.
[0065] The chemical composition and mass percentage of the red mud are: SiO 2 11.38%, CaO20.21%, MgO1.12%, A1 2 O 3 32.24%, Fe 2 O 3 6.98%, K 2 O 0.47%, Na 2 O 3.75%, the remainder is impurities.
[0066] The chemical composition and mass percentage of the electric furnace slag are: CaO 36.27%, Fe 2 O 3 39.44%, SiO 2 10.89%, MgO 3.11%, MnO 3.20%, P 2 O 5 1.03%, A l 2 O 3 4.28%, the remainder is impurities.
[0067] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), PF = 0.7149 (rounded); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.3839 (rounded);
[0068] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2+A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0069] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0070] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0071] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0072] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0073] Embodiment 3:
[0074] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0075] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0076] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 4:1.
[0077] The chemical composition and mass percentage of the red mud are: SiO 211.38%, CaO20.21%, MgO1.12%, A1 2 O 3 32.24%, Fe 2 O 3 6.98%, K 2 O 0.47%, Na 2 O 3.75%, the remainder is impurities.
[0078] The chemical composition and mass percentage of the electric furnace slag are: CaO 36.27%, Fe 2 O 3 39.44%, SiO 2 10.89%, MgO 3.11%, MnO 3.20%, P 2 O 5 1.03%, A l 2 O 3 4.28%, the remainder is impurities.
[0079] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), PF = 0.7615 (rounded); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.4343 (rounded);
[0080] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0081] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0082] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0083] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0084] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0085] Embodiment 4:
[0086] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0087] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0088] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 3:1.
[0089] Furthermore, the chemical composition and mass percentage of the red mud are: SiO 2 11.78%, CaO20.98%, MgO 1.12%, A1 2 O 3 33.24%, Fe 2 O 3 7.54%, K 2 O 0.49%, Na 2 O 3.55%, the remainder is impurities.
[0090] The chemical composition and mass percentage of the electric furnace slag are: CaO 37.27%, Fe 2 O 3 37.56%, SiO 2 9.89%, MgO 3.15%, MnO 3.32%, P2 O 5 1.05%、Al 2 O 3 4.79%, the remainder is impurities.
[0091] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), PF = 0.7503 (rounded off); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.4181 (rounded);
[0092] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0093] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0094] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0095] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0096] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0097] Embodiment 5:
[0098] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0099] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0100] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 2:1.
[0101] Furthermore, the chemical composition and mass percentage of the red mud are: SiO 2 11.78%, CaO20.98%, MgO 1.12%, A1 2 O 3 33.24%, Fe 2 O 3 7.54%, K 2 O 0.49%, Na 2 O 3.55%, the remainder is impurities.
[0102] The chemical composition and mass percentage of the electric furnace slag are: CaO 37.27%, Fe 2 O 3 37.56%, SiO 2 9.89%, MgO 3.15%, MnO 3.32%, P 2 O 5 1.05%、Al 2 O 3 4.79%, the remainder is impurities.
[0103] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), PF = 0.7230 (rounded off); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3), CRF = 0.3874 (rounded);
[0104] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0105] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0106] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0107] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0108] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0109] Embodiment 6:
[0110] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0111] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0112] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 4:1.
[0113] Furthermore, the chemical composition and mass percentage of the red mud are: SiO 2 11.78%, CaO20.98%, MgO 1.12%, A1 2 O 3 33.24%, Fe 2 O 3 7.54%, K 2 O 0.49%, Na 2 O 3.55%, the remainder is impurities.
[0114] The chemical composition and mass percentage of the electric furnace slag are: CaO 37.27%, Fe 2 O 3 37.56%, SiO 2 9.89%, MgO 3.15%, MnO 3.32%, P 2 O 5 1.05%、Al 2 O 3 4.79%, the remainder is impurities.
[0115] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), PF = 0.7671 (rounded off); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.4360 (rounded);
[0116] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0117] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0118] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0119] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0120] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0121] Embodiment 7:
[0122] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 44 parts of ordinary cement, 20 parts of electric furnace slag-red mud mixed slag, 110 parts of sand, 10 parts of double-fast cement, 10 parts of silica fume, 1 part of water reducing agent, 12 parts of expansion agent and 30 parts of water.
[0123] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0124] The mass ratio of the mixture of 700-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 700-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 3:1.
[0125] The chemical composition and mass percentage of the red mud are: SiO 2 11.38%, CaO20.21%, MgO1.12%, A1 2 O 3 32.24%, Fe 2 O 3 6.98%, K 2 O 0.47%, Na 2O 3.75%, the remainder is impurities.
[0126] The chemical composition and mass percentage of the electric furnace slag are: CaO 36.27%, Fe 2 O 3 39.44%, SiO 2 10.89%, MgO 3.11%, MnO 3.20%, P 2 O 5 1.03%, A l 2 O 3 4.28%, the remainder is impurities.
[0127] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), PF = 0.7437 (rounded off); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.4158 (rounded);
[0128] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0129] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0130] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0131] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0132] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0133] Comparative Example 1:
[0134] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0135] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0136] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 1:1.
[0137] The chemical composition and mass percentage of the red mud are: SiO 2 11.38%, CaO20.21%, MgO1.12%, A1 2 O 3 32.24%, Fe 2 O 3 6.98%, K 2 O 0.47%, Na 2 O3.75%, the remainder is impurities.
[0138] The chemical composition and mass percentage of the electric furnace slag are: CaO 36.27%, Fe 2 O 3 39.44%, SiO 2 10.89%, MgO 3.11%, MnO 3.20%, P 2 O 5 1.03%, A l 2 O 3 4.28%, the remainder is impurities.
[0139] Performance factor PF=M(CaO+SiO 2 +A12 O 3 ) / M(red mud + electric furnace slag), PF = 0.6712 (rounded off); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.3224 (rounded off);
[0140] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0141] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0142] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0143] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0144] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0145] Comparative Example 2:
[0146] A low-carbon electric furnace slag-red mud-based cement ink material comprises the following components in parts by weight: 39 parts of ordinary cement, 25 parts of electric furnace slag-red mud mixed slag, 105 parts of sand, 7 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0147] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0148] The mass ratio of the mixture of 600-mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 600-mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is 5:1.
[0149] The chemical composition and mass percentage of the red mud are: SiO 2 11.38%, CaO20.21%, MgO1.12%, A1 2 O 3 32.24%, Fe 2 O 3 6.98%, K 2 O 0.47%, Na 2 O3.75%, the remainder is impurities.
[0150] The chemical composition and mass percentage of the electric furnace slag are: CaO 36.27%, Fe 2 O 3 39.44%, SiO 2 10.89%, MgO 3.11%, MnO 3.20%, P 2 O 5 1.03%, A l 2 O 3 4.28%, the remainder is impurities.
[0151] Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud + electric furnace slag), PF = 0.7786 (rounded off); carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), CRF = 0.4478 (rounded);
[0152] Where: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content; M(CaO+SiO 2+A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 M (red mud + electric furnace slag) is the total content of the mixed slag.
[0153] The above-mentioned low-carbon electric furnace slag-red mud-based cement ink material has the following specific steps:
[0154] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume, expansion agent and water reducer are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0155] 2) The electric furnace slag and red mud are fully mixed and added to the basic mixture in batches, and stirred to obtain a mixture precursor. In terms of weight percentage, 30% is added for the first time, 30% is added for the second time, and 40% is added for the third time. The stirring speed for each addition is 150 rpm and the stirring time is 420 s.
[0156] 3) adding water in batches to the mixture precursor for mixing and stirring, the first time 50% of the water is added, the stirring time is 60s, the mixing and stirring speed is 250rpm, and the second time the remaining water is added, the stirring time is 420s, and the mixing and stirring speed is 450rpm, to obtain an electric furnace slag-red mud based cement ink material.
[0157] Comparative Example 3:
[0158] A common cement ink material comprises the following components in parts by weight: 64 parts of common cement, 105 parts of sand, 10 parts of double-fast cement, 7 parts of silica fume, 0.8 parts of water reducer, 9 parts of expansion agent and 25 parts of water.
[0159] Ordinary cement is PO 42.5 ordinary silicate cement; double fast cement is sulphoaluminate cement; silica fume SiO 2 The content is 94%; the particle size of quartz sand is 0.075-0.5mm; the water reducing agent is a solid powder type polycarboxylic acid high-efficiency water reducing agent with a water reducing efficiency of 20%; the water is ordinary tap water; the expansion agent is UEA type concrete expansion agent (powder).
[0160] The above-mentioned ordinary cement ink material, the specific steps are as follows:
[0161] 1) Ordinary Portland cement, sulphoaluminate cement, quartz sand, silica fume and expansion agent are mixed and stirred at a stirring speed of 150 rpm for 180 s to obtain a basic mixture.
[0162] 2) After mixing water and a water reducing agent, add them to the base mixture in batches for mixing and stirring. The first time 50% of the water and the water reducing agent are added, the stirring time is 60s and the mixing and stirring speed is 250rpm. The second time the remaining amount of water and the water reducing agent are added, the stirring time is 420s and the mixing and stirring speed is 450rpm to obtain an ordinary cement ink material.
[0163] The electric furnace slag-red mud-based cement ink materials configured in Examples 1-7 and other cement ink materials configured in Comparative Examples 1-3 were mixed, respectively, and cast into standard test blocks of 70.7 mm × 70.7 mm × 70.7 mm through a mortar consistency tester, and then cured in a steam curing room for 3 days and 28 days, and then a cube compression test was performed, and the test conditions of all the test pieces were exactly the same. The test results are shown in the table.
[0164] Table: Test results of Examples 1-7 and Comparative Examples 1-3 test pieces:
[0165]
[0166] According to experiments, the recommended consistency of the ink material used for architectural 3D printing is 50-80 mm. This embodiment can be used in the architectural 3D printing industry.
[0167] As shown in Table 1, the low-carbon electric furnace slag-red mud-based cement ink material proposed in this embodiment has a reduced consistency, indicating that it has better fluidity and is more conducive to the discharge of materials from the 3D printing outlet. After oxygen-enhanced curing, its 3d cube compressive strength increases by 20% to 40%, and the 28d cube compressive strength does not change much.
[0168] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A low-carbon electric furnace slag-red mud-based cement ink material, It is characterized in that The ink material comprises the following components in parts by weight: 34-44 parts of ordinary cement, 20-30 parts of electric furnace slag-red mud mixed slag, 100-110 parts of sand, 4-10 parts of double-fast cement, 4-10 parts of silica fume, 0.6-1.0 parts of water reducing agent, 6-12 parts of expansion agent and 20-30 parts of water.
2. A low-carbon electric furnace slag-red mud-based cement ink material according to claim 1, It is characterized in that The mass ratio of the mixture of 500-700 mesh red mud ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag-red mud mixed slag and 500-700 mesh electric furnace slag ultrafine powder obtained by ultrafine tire vertical milling the electric furnace slag is (2-4):
1.
3. A low-carbon electric furnace slag-red mud-based cement ink material according to claim 2, It is characterized in that The red mud is ultrafine red mud powder obtained by vertical grinding with ultrafine tires to a size of 500-700 meshes, and the chemical composition and mass percentage are as follows: SiO 2 11.26%~12.21%, CaO 19.76%~21.30%, MgO 0.85%~1.46%, A1 2 O 3 31.29%~33.60%, Fe 2 O 3 6.38%~10.02%, K 2 O 0.36%~0.62%, Na 2 O 2.35%~4.20%, the remainder is impurities; The electric furnace slag is an electric furnace slag ultrafine powder obtained by ultrafine tire vertical grinding to 500-700 meshes, and its chemical composition and mass percentage are as follows: CaO 34.13-38.34%, Fe 2 O 3 34.42%~43.01%,SiO 2 9.42%~12.57%, MgO2.11%~4.12%, MnO 3.01%~4.42%, P 2 O 5 0.64%~1.43%,Al 2 O 3 4.01%~5.91%, the remainder is impurities; Performance factor PF=M(CaO+SiO 2 +A1 2 O 3 ) / M(red mud+electric furnace slag), 0.714≤PF≤0.768; Carbon reduction factor CRF = M(A1 2 O 3 ) / M(CaO+SiO 2 +A1 2 O 3 ), 0.383≤CRF≤0.436; in: M(A1 2 O 3 ) is A1 in mixed slag 2 O 3 Total content of M(CaO+SiO 2 +A1 2 O 3 ) is CaO, SiO in the mixed slag 2 、A1 2 O 3 Total content of M (red mud + electric furnace slag) is the total content of the mixed slag.
4. A low-carbon electric furnace slag-red mud-based cement ink material according to claim 1, It is characterized in that The sand includes quartz sand and / or machine-made sand, with a particle size of 0.075 to 0.5 mm; The ordinary cement is ordinary Portland cement with a strength of 42.5; The silica fume is microsilica powder SiO 2 The content is 92% to 98%; The water reducer is a polycarboxylate water reducer in the form of powder; The double-fast cement is sulphoaluminate cement; The expansion agent is a UEA concrete expansion agent, and the material form is powder; The water is tap water.
5. A method for preparing the low-carbon electric furnace slag-red mud-based cement ink material according to any one of claims 1 to 4, It is characterized in that The following steps are involved: 1) Mix ordinary cement, double-fast cement, silica fume, sand, expansion agent and water reducing agent to obtain a basic mixture: 2) fully mixing the electric furnace slag and the red mud and adding them to the basic mixture in batches to obtain a mixture precursor; 3) adding water in batches to the mixture precursor for mixing and stirring to obtain a low-carbon electric furnace slag-red mud-based cement ink material.
6. The method for preparing a low-carbon electric furnace slag-red mud-based cement ink material according to claim 5, It is characterized in that In step 1), the mixing and stirring speed is 100-200 rpm, and the time is 120-300 s.
7. The method for preparing a low-carbon electric furnace slag-red mud-based cement ink material according to claim 5, It is characterized in that Step 2) When the electric furnace slag and red mud are mixed, the stirring speed is 100-150 rpm and the stirring time is 120-180 s; The stirring speed for each addition is 100-200 rpm, and the stirring time after each addition is 180-420 s.
8. The method for preparing a low-carbon electric furnace slag-red mud-based cement ink material according to claim 6, It is characterized in that In step 3), 50% of water is first added to the mixture precursor for mixing and stirring at a stirring speed of 100-200 rpm for 60-180 seconds.
9. The method for preparing a low-carbon electric furnace slag-red mud-based cement ink material according to claim 6, It is characterized in that In step 3), 50% of water is added to the mixture precursor for mixing and stirring at a stirring speed of 300 to 500 rpm for 300 to 600 seconds.
10. An application of the low-carbon electric furnace slag-red mud-based cement ink material as claimed in claim 1, 2, 3 or 4, It is characterized in that The ink material is applied to 3D printing building materials, and the printed components are subjected to steam curing.
Citation Information
Patent Citations
Composite cementitious material, and preparation method and application of composite cementitious material
CN110330282A
Low-shrinkage 3D printing concrete co-doped with lignin fibers and preparation method of low-shrinkage 3D printing concrete
CN113372074A
Cement admixture using superfine tire vertical mill steel slag instead of mineral powder and preparation method thereof
CN115353310A
Application method of red mud in 3D printing
CN118108466A
Inorganic quick setting composition using electric furnace molten slag, method of producing same, and method of constructing same
KR101370609B1