Ecological low-temperature fired coal gangue-based porous ceramic material and preparation method thereof
By firing coal gangue-based porous ceramic materials at low temperature, using a combination of polystyrene, soluble starch and glass powder, combined with diatomaceous earth to optimize the pore gradation, the problem of water volatilization in sandy and saline-alkali soils is solved, and high water absorption and long-lasting properties are achieved. It has long-term water retention performance, is suitable for ecological restoration and reduces production costs.
Patent Information
- Application Number
- CN202410762642.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-13
AI Technical Summary
In ecological restoration of desertified areas, sandy lands, and saline-alkali lands, the low plant survival rate is mainly due to the problem of water volatilization. The existing ceramsite covering and water-retaining agents have problems such as high cost, low water absorption rate, or attenuation of water absorption capacity caused by salt.
The coal gangue-based porous ceramic material is fired at low temperature, and a combination of polystyrene, soluble starch and glass powder is used to form a material with high porosity and strong water permeability. Diatomaceous earth is used to optimize the pore gradation to improve water absorption and water retention properties. Avoid the effects of salt.
It achieves high water absorption and long-term water retention performance, has strong material reusability, is suitable for sandy land restoration, improves plant survival rate, and reduces production costs and energy consumption.
Smart Images

Figure CN118754603A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous ceramic material preparation, and in particular to an ecological low-temperature fired coal gangue-based porous ceramic material and a preparation method thereof. Background Art
[0002] At present, ecological restoration in desertified areas, sandy land, degraded sandy grassland and saline-alkali land is faced with the problem of low survival rate of plant species. One of the main reasons is that water evaporates before it can be absorbed by plant roots. Therefore, water-saving and drought-resistant, rational and efficient use of limited water resources are key issues that must be solved in the ecological restoration of sandy land. At present, in order to solve this problem, ceramsite covering, mulch covering and adding water retaining agent to the soil are used to delay water volatilization. However, the preparation and maintenance time of ceramsite is very long, usually 14-30 days, and the water absorption rate of most ceramsite is very low, only about 30%, which cannot store water well. On the one hand, the cost of using mulch covering is high, and the waste mulch is easy to pollute the environment, and it will also affect safety in extreme weather. Although adding water retaining agent can alleviate soil water loss to a great extent, the water retaining agent will cause the water absorption capacity to decay quickly due to the effect of salt during use (especially in saline-alkali land). Therefore, a material with low cost, high water absorption rate and strong water retention capacity is needed to play a role in ecological restoration of sandy land, retain soil moisture and improve the survival rate of plants.
[0003] Coal gangue is a bulk solid waste with the characteristics of large reserves and low price, which can reduce costs. Porous ceramic materials have high porosity, low density, and high specific surface area, and are widely used in catalytic carrier materials, filter materials, sound absorbing materials, thermal insulation materials and other fields. Preparing coal gangue into porous materials can not only broaden the application scope of coal gangue and make high value-added use of it, but also apply porous materials to sandy land and ecological restoration, reduce soil moisture loss, conserve water and resist drought, and improve the survival rate of plants.
[0004] Although the porous ceramic materials currently prepared from coal gangue have various excellent properties and a wide range of applications, most ceramic materials have the problem of high sintering temperature (generally above 1000°C) and the water absorption rate is not high enough. Summary of the invention
[0005] The purpose of the present invention is to provide an ecological low-temperature fired coal gangue-based porous ceramic material and a preparation method thereof. The prepared porous ceramic material has high porosity, strong water permeability, can play a humidifying role, and has higher reuse capacity. The water absorption capacity will not be reduced due to the effect of salt. After absorbing water, due to the action of capillary forces, it can delay water evaporation and improve the water retention performance of the material.
[0006] To achieve the above object, the present invention provides a method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material, comprising the following steps:
[0007] Step 1: Raw material preparation and pretreatment;
[0008] Step 2: preparing slurry;
[0009] Step 3: pour the slurry into a mold and place it in a drying oven to dry and shape the desired embryo;
[0010] Step 4: Place the embryo body in a furnace for sintering, and after sintering, cool the furnace to room temperature to obtain a coal gangue-based porous ceramic material.
[0011] Preferably, the specific operation of step 1 is: preparing polystyrene, grinding the prepared polystyrene into powder using a mortar, crushing the coal gangue, drying and sieving.
[0012] Preferably, the specific operation of step 2 is: uniformly mix coal gangue, soluble starch, glass powder and diatomaceous earth in a certain proportion, add appropriate amount of water and stir evenly to form slurry.
[0013] Preferably, the mesh size of the coal gangue is 100-200 mesh, and the drying temperature is 60-80°C.
[0014] Preferably, the drying temperature is 60°C.
[0015] Preferably, the contents of the components in step 2 are: 33%-44% coal gangue, 12%-24% polystyrene, 16%-25% soluble starch, 18%-31% glass powder, and 0-5% diatomaceous earth.
[0016] Preferably, the sintering in step 4 is carried out in an air atmosphere at a heating rate of 2-5°C / min, the sintering temperature is 600-650°C, and the sintering time is 1-2h.
[0017] Preferably, the sintering heating rate is 3°C / min and the sintering temperature is 600°C.
[0018] The invention also provides a gangue-based porous ceramic material prepared by the preparation method.
[0019] In the sintering process of the present invention, the combustibles in soluble starch, polystyrene and coal gangue will be burned out. Both soluble starch and polystyrene are main pore-forming agents. After the carbon in the coal gangue is burned out, fine channels and tiny pores will be left in situ. These three components can form different holes during the sintering process, and the gradation is formed according to the different hole sizes. Diatomaceous earth itself has a large number of micron-sized holes, which can further optimize the hole gradation formed by starch and the like, and improve the water absorption and water retention of ceramic materials.
[0020] The present invention selects soluble starch, on the one hand as a pore-forming agent, and on the other hand as a binder when configuring the slurry, so that the embryo has a stable shape during sintering. Polystyrene is used as a pore-forming agent, which can form spherical holes after burning out, and there is little residue after burning out. Coal gangue itself contains a certain amount of combustibles that can be used as a pore-forming agent to form a certain amount of tiny pores. In addition, it can work together with glass powder to form a ceramic material skeleton. Glass powder is the main binder of ceramic materials. During sintering, it forms a skeleton with coal gangue, so that the embryo has a certain strength, and the pore structure can be retained after firing. The pores of diatomaceous earth itself still exist after firing, and are embedded in the ceramic skeleton, forming a gradation with the pores formed by the pore-forming agent, which greatly improves the water absorption rate of the material. After absorbing water, due to the action of capillary forces, it can delay the evaporation of water and improve the water retention performance of the material.
[0021] The present invention uses coal gangue as the main matrix, polystyrene beads and soluble starch as templates, and adopts a low-temperature (600-650°C) sintering method to prepare coal gangue into porous ceramic materials, giving coal gangue high added value. At the same time, the porous ceramics prepared from coal gangue have the characteristics of high porosity and large specific surface area, and by adjusting the internal pore size gradation of the porous ceramics, porous ceramics with higher water absorption rate and stronger water retention performance are obtained. It is used as an ecological restoration material for desertified areas, sandy land, degraded sandy grassland, saline-alkali land, etc., to reduce soil water loss and play a moisturizing role. The porous ceramic has a high porosity and a strong water seepage effect, which can play a humidifying role. In addition, compared with agricultural water retaining agents, porous ceramic materials have a higher reuse capacity, and the water absorption capacity will not be reduced due to the effect of salt. The application of coal gangue in agricultural water retention can not only consume solid waste coal gangue, but also be green and environmentally friendly.
[0022] Therefore, the present invention adopts the above-mentioned ecological low-temperature fired coal gangue-based porous ceramic material and its preparation method, which has the following beneficial effects:
[0023] (1) The present invention prepares a porous ceramic material with high water absorption and high water retention effect. The 24-hour water absorption rate of the porous ceramic can be as high as 164%. In a dry indoor environment, it can retain water for 9 hours, and in a constant temperature and humidity environment with a temperature of 25°C and a humidity of 93%, it can retain water for 43 hours. It can absorb water quickly and release water at a stable rate.
[0024] (2) The porous ceramic was immersed in pure water and 0.9% NaCl solution for 24 hours respectively, and then dried in a forced air drying oven at 60°C to constant weight. The water absorption rate did not decrease after repeating the process for 5 times.
[0025] (3) The preparation method of the present invention is simple and efficient, with low sintering temperature and low energy consumption. In addition, the use of solid waste coal gangue as the main raw material can broaden the application scope of coal gangue and make high value-added use of it.
[0026] (4) The strength of conventional porous ceramics is very high, which is not conducive to the growth of plant roots. The porous ceramics of the present invention have moderate strength, and the roots can directly pass through the porous ceramics, which is more conducive to the growth of the roots.
[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a preparation process flow chart of an ecological low-temperature fired coal gangue-based porous ceramic material and a preparation method thereof according to Embodiment 1 and Embodiment 2 of the present invention;
[0029] Figure 2 This is a cross-sectional scanning electron microscope image of a porous ceramic material of Example 1 of an ecological low-temperature fired coal gangue-based porous ceramic material and a preparation method thereof of the present invention;
[0030] Figure 3 This is a cross-sectional scanning electron microscope image of the porous ceramic material of Example 3 of a raw low-temperature fired coal gangue-based porous ceramic material and a preparation method thereof of the present invention. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0032] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0033] Example
[0034] The present invention provides a method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material, comprising the following steps:
[0035] Step 1, raw material preparation and pretreatment: prepare polystyrene, grind the prepared polystyrene into powder with a mortar, crush the coal gangue, dry and sieve. The mesh number of the coal gangue is 100-200 mesh, the drying temperature is 60-80°C, and the preferred drying temperature is 60°C.
[0036] Step 2: Prepare slurry; mix coal gangue, soluble starch, glass powder and diatomaceous earth in a certain proportion, add appropriate amount of water and stir evenly to form slurry. The content of each component is: 33%-44% coal gangue, 12%-24% polystyrene, 16%-25% soluble starch, 18%-31% glass powder, 0-5% diatomaceous earth. The microstructure of polystyrene is a 0.2μm sphere and the pores remaining after burning are spherical, which can store more water.
[0037] Soluble starch is a pore former on the one hand, and a binder when preparing the slurry on the other hand, so that the embryo has a stable shape during sintering. Polystyrene is a pore former, which can form spherical cavities after sintering, and there is little residue after sintering. Coal gangue itself contains a certain amount of combustibles that can be used as a pore former to form a certain amount of tiny pores. In addition, it can work together with glass powder to form the skeleton of ceramic materials. Glass powder is the main binder of ceramic materials. During sintering, it works together with coal gangue to form a skeleton, so that the embryo has a certain strength, and the pore structure can be retained after firing. The cavities of diatomaceous earth itself still exist after firing and are embedded in the ceramic skeleton. They form a graded distribution with the cavities formed by the pore former, which greatly improves the water absorption rate of the material. After absorbing water, due to the action of capillary forces, it can delay the evaporation of water and improve the water retention performance of the material.
[0038] Step 3: pour the slurry into a mold and place it in a drying oven to dry and shape the desired embryo;
[0039] Step 4: Place the embryo in a furnace and heat it at a rate of 2-5°C / min in an air atmosphere. The sintering temperature is 600-650°C and the sintering time is 1-2h. After sintering, cool it to room temperature to obtain a coal gangue-based porous ceramic material. Preferably, the sintering heating rate is 3°C / min and the sintering temperature is 600°C.
[0040] Example 1
[0041] like Figure 1 As shown, the present invention provides a method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material, the raw materials and mass percentage composition are: 33% coal gangue, 24% polystyrene, 25% soluble starch, and 18% glass powder. The preparation process is: crush the coal gangue and pass it through a 200-mesh sieve. Grind the prepared polystyrene into powder with a mortar and pestle, and also pass it through 200 mesh. Then mix all the substances evenly according to the proportion, add a certain amount of ultrapure water to form a ceramic slurry, and use a glass rod to fully stir until the slurry is evenly mixed. After the mixed slurry is poured into a mold for forming, it is placed in a blast drying oven and dried at 60°C for 12 hours until the blank is completely dry. Finally, the blank is placed in a tubular furnace, heated to 610°C at a rate of 3°C / min and sintered for 2 hours to obtain a water-absorbing and water-retaining porous ceramic material.
[0042] like Figure 2 As shown, the porous ceramics prepared by using the above raw material ratios have different pore size distributions due to the use of pore-forming agents with different particle sizes. The water absorption rate of the water-absorbing and water-retaining porous ceramic material prepared is 91.1% in 24 hours, the water is completely lost in 430 minutes in a dry indoor environment, and the water is retained for 25 hours in a constant temperature and humidity environment with a temperature of 25°C and a humidity of 93%.
[0043] Example 2
[0044] like Figure 1 As shown, the present invention provides a method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material, the raw materials and mass percentage composition are: 33% coal gangue, 24% polystyrene, 16% soluble starch, and 27% glass powder. The preparation process is: crush the coal gangue and pass it through a 200-mesh sieve. Grind the prepared polystyrene into powder with a mortar and pestle, and also pass it through 200 mesh. Then mix all the substances evenly according to the proportion, add a certain amount of ultrapure water to form a ceramic slurry, and use a glass rod to fully stir until the slurry is evenly mixed. After the mixed slurry is poured into a mold for forming, it is placed in a blast drying oven and dried at 60°C for 12 hours until the blank is completely dry. Finally, the blank is placed in a tubular furnace, heated to 600°C at a rate of 3°C / min and sintered for 2 hours to obtain a water-absorbing and water-retaining porous ceramic material.
[0045] The water absorption rate of the water-absorbing and water-retaining porous ceramic material was 67% in 24 hours, the water was completely lost in 271 minutes in a dry indoor environment, and the water was retained for 17 hours in a constant temperature and humidity environment of 25°C and 93% humidity.
[0046] Example 3
[0047] A low-temperature fired coal gangue-based porous ceramic material for ecological use, the raw materials and mass percentage composition are: 35% coal gangue, 13% polystyrene, 18% soluble starch, 29.5% glass powder, and 4.5% diatomaceous earth. The preparation process is: crush the coal gangue and pass it through a 200-mesh sieve. Grind the prepared polystyrene into powder with a mortar and pestle, and also pass it through 200 mesh. Then all the substances are mixed evenly according to the proportion, a certain amount of ultrapure water is added to form a ceramic slurry, and a glass rod is used to fully stir until the slurry is mixed evenly. After the mixed slurry is poured into a mold for forming, it is placed in a blast drying oven and dried at 60°C for 12 hours until the blank is completely dry. Finally, the blank is placed in a tubular furnace, heated to 600°C at a rate of 3°C / min and sintered for 2 hours to obtain a water-absorbing and water-retaining porous ceramic material.
[0048] like Figure 3 As shown, the added diatomite is embedded in the porous ceramic in the form of small particles, and the tiny pores on the surface of the diatomite particles further optimize the pore structure of the porous ceramic. The water absorption rate of the water-absorbing and water-retaining porous ceramic material prepared using the raw material ratio of this embodiment is 164% in 24 hours. In a dry indoor environment, the water is completely lost in 575 minutes, and the water is retained for 43 hours in a constant temperature and humidity environment with a temperature of 25°C and a humidity of 93%.
[0049] Therefore, the present invention adopts the above-mentioned ecological low-temperature fired coal gangue-based porous ceramic material and its preparation method. The prepared porous ceramic material has high porosity, strong water permeability, can play a humidifying role, and has higher reuse capacity. The water absorption capacity will not be reduced due to the action of salt. After absorbing water, due to the action of capillary force, it can delay water evaporation and improve the water retention performance of the material.
[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing ecological low-temperature fired coal gangue-based porous ceramic materials, Features: The following steps are involved: Step 1: Raw material preparation and pretreatment; Step 2: preparing slurry; Step 3: pour the slurry into a mold and place it in a drying oven to dry and shape the desired embryo; Step 4: Place the embryo body in a furnace for sintering, and after sintering, cool the furnace to room temperature to obtain a coal gangue-based porous ceramic material.
2. The method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material according to claim 1, Features: The specific operation of the step 1 is: preparing polystyrene, grinding the prepared polystyrene into powder using a mortar, crushing the coal gangue, drying and sieving.
3. The method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material according to claim 1, Features: The specific operation of the step 2 is: uniformly mix the coal gangue, soluble starch, glass powder and diatomaceous earth in a certain proportion, add appropriate amount of water and stir evenly to form a slurry.
4. The method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material according to claim 2, Features: The mesh number of the coal gangue is 100-200 meshes, and the drying temperature is 60-80°C.
5. The method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material according to claim 4, Features: The drying temperature is 60°C.
6. The method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material according to claim 3, Features: The contents of the components in step 2 are: 33%-44% of coal gangue, 12%-24% of polystyrene, 16%-25% of soluble starch, 18%-31% of glass powder, and 0-5% of diatomaceous earth.
7. The method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material according to claim 1, Features: In the step 4, the sintering is carried out in an air atmosphere at a heating rate of 2-5°C / min, the sintering temperature is 600-650°C, and the sintering time is 1-2h.
8. The method for preparing an ecological low-temperature fired coal gangue-based porous ceramic material according to claim 7, Features: The sintering heating rate is 3°C / min, and the sintering temperature is 600°C.
9. An ecological low-temperature fired coal gangue-based porous ceramic material, Features: The gangue-based porous ceramic material is prepared by the preparation method described in any one of claims 1-8.
Citation Information
Patent Citations
Porous ceramic material with high water absorption rate and high water retention rate and preparation method and application thereof
CN107586150A
Microcrystalline composite coal gangue based foamed ceramic thermal insulation board, and preparation method thereof
CN110395969A
Coal gangue mixed firing method
CN117510116A
Microbial flora carrier as well as preparation method and application thereof
CN117866938A
Method for preparing recrystallized SIC high temperature gas filter element
CN1821180A
Cited By
Coal gangue-based porous material as well as preparation method and application thereof in ecological restoration
CN120004648A
Porous spongy honeycomb carbon material and preparation method thereof
CN121318532A
High-water-absorption and high-strength porous ceramic based on solid waste and preparation method thereof