High-energy-storage-density multiphase ceramic material with internal crystal structure and preparation method of high-energy-storage-density multiphase ceramic material
By controlling the precipitation behavior of CaTiO3 in the BaTiO3-BaZrO3-CaTiO3 system, an endocrystalline multi-phase ceramic material is designed, which solves the problem of low energy storage density of dielectric capacitors and achieves an increase in high-efficiency energy storage density and efficiency. It is suitable for ceramics Capacitor dielectric energy storage.
Patent Information
- Application Number
- CN202410921918.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The energy storage density of existing dielectric capacitors is small, making it difficult to meet the needs for miniaturization, integration, and lightweighting of electronic equipment. BaTiO3 is prone to saturation polarization under low electric fields and has low breakdown electric field strength, which limits its energy storage density. and improvement of energy storage efficiency.
In the BaTiO3-BaZrO3-CaTiO3 ternary complex phase system, by controlling the precipitation behavior of CaTiO3, a complex phase ceramic material with an endocrystalline structure is designed, which enhances the breakdown electric field strength and maintains high dielectric constant and polarization difference, forming A combination of 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3, the material is prepared by traditional solid-phase sintering method.
Achieving high effective energy storage density and energy storage efficiency, the breakdown electric field strength reaches 553.9kV/cm, the polarization difference is 30.77μC/cm2, the effective energy storage density reaches 5.86J cm-3, and the energy storage efficiency reaches 86.7%. Has excellent dielectric capacitor energy storage performance.
Smart Images

Figure BDA0004936958520000061 
Figure FDA0004936958500000011 
Figure FDA0004936958500000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electronic ceramic materials, and in particular relates to a multiphase ceramic material with an internal crystalline structure and high energy storage density which can be applied to dielectric energy storage of ceramic capacitors, and a preparation method thereof. Background Art
[0002] The efficient use of various energy sources in today's society depends on the development of advanced energy storage technology. Compared with common electrochemical energy storage technology, electrostatic energy storage technology with dielectric capacitors as core components has many advantages such as ultra-fast charging and discharging speed, high power density and excellent cycle life. Although electrostatic energy storage capacitors have been partially used in pulse power electronic equipment in the military, medical and nuclear energy fields, the energy storage density of dielectric capacitors is relatively small. In actual application, they usually require a larger mass and volume, which cannot meet the needs of miniaturization, integration and lightweight of electronic equipment. Therefore, optimizing the energy storage performance of dielectric capacitors is a must for the development of new generation electronic component materials.
[0003] For dielectric materials, their energy storage function is achieved through dielectric polarization (P) in an external electric field (E), that is, dielectric energy storage materials store energy through dielectric polarization and separation of positive and negative charges under an external electric field. For dielectric energy storage materials, the total energy storage density Effective energy storage density Energy storage efficiency The basic performance requirement of pulse capacitors for dielectric materials is to have high effective energy storage density W rec and high energy storage efficiency η. In the above formula, P max and P r They are the maximum polarization during charging and the residual polarization during discharging, and E is the external electric field. It can be seen from the formula that the dielectric material has a large polarization difference △P(P max -P r ), delayed saturation polarization and high breakdown electric field strength (E b ) is conducive to the capacitor to obtain excellent energy storage performance.
[0004] BaTiO3 has become the world's most widely used commercial ferroelectric capacitor ceramic due to its stable perovskite structure and intrinsic high dielectric constant. It is often used to manufacture Electronic Industries Alliance (EIA) Class II X7R or X8R multilayer ceramic capacitors (MLCC) by doping or forming solid solutions with other components. However, BaTiO3 is prone to form saturation polarization under low electric fields, and has problems such as low breakdown electric field strength and high residual polarization, which limits its energy storage density and energy storage efficiency, making it difficult to apply to pulse energy storage capacitors. By constructing 0-3 type composite ceramics, that is, introducing low dielectric and high insulating materials such as aluminum oxide, aluminum nitride, and magnesium oxide into the perovskite ferroelectric matrix, it has been proven that the electrical breakdown strength (E b ) and reduce residual polarization. However, the formation of the existing 0-3 type multiphase structure of such materials requires the addition of a large amount of low-dielectric and high-insulation materials as the second phase. These second phases mainly exist at the ceramic grain boundaries, which greatly weaken the dielectric constant and polarization difference △P of the material, and thus the effect of improving the energy storage density of the material is very limited. Therefore, if the energy storage characteristics of multiphase ceramics are to be enhanced, it is necessary to find new material design methods to control the content and location of the second phase, while ensuring the enhanced breakdown electric field strength (E b ) while still maintaining a relatively high dielectric constant and polarization difference △P.
[0005] In summary, in the present invention, a novel design method for composite ceramic materials with high energy storage density and internal crystalline structure is proposed, and excellent comprehensive energy storage characteristics are obtained in the BaTiO3-BaZrO3-CaTiO3 ternary composite system (abbreviated as BCZT). Different from the idea of forming the second phase at the grain boundary by adding the second component in the conventional 0-3 type composite ceramic design, the formation of the second phase of the composite material in the present invention originates from the intracrystalline self-precipitation behavior of the designed system. Because CaTiO3 has a limited solid solubility in the BaTiO3 matrix, it is beneficial to control the intracrystalline precipitation behavior of the appropriate amount of CaTiO3 second phase through precise composition adjustment, thereby achieving the purpose of enhancing the breakdown electric field strength and maintaining a high dielectric constant. At the same time, BaZrO3 can form an infinite solid solution with BaTiO3, and because of the difference in the radius and ferroelectric activity of the perovskite B-site ion, the relaxation characteristics of the material and the polarization difference △P can be enhanced. Among them, the best sample 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3 with an internal crystal structure not only has a higher breakdown electric field strength (E b =553.9kV / cm), and also has a high polarization difference △P (30.77μC / cm 2 ), and obtained W rec =5.86Jcm -3 , with excellent performance of η=86.7%, it has great application potential in the field of dielectric capacitor energy storage. Summary of the invention
[0006] The characteristic of the present invention is that an endocrystal second phase BCZT high energy storage density composite ceramic material is designed, taking into account the rich multi-scale design factors in the BaTiO3-BaZrO3-CaTiO3 system, that is, the combination of BaTiO3 and BaZrO3 can enhance the dielectric relaxation behavior, and the limited solid solubility of CaTiO3 in the BaTiO3 matrix is conducive to controlling the precipitation behavior of the second phase. Through fine component control, a BCZT composite material with an endocrystal second phase structure with an appropriate amount of CaTiO3 precipitated is constructed, so as to achieve the enhancement of E while maintaining a high polarization difference △P. b goal.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A high energy storage density multiphase ceramic material with an internal crystalline structure, characterized in that the component design is: The value of x is 0.21-0.9. Through composition refinement and process exploration, the preferred composition is x=0.65, i.e. 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3. This sample has a special internal crystal structure and its performance can reach: effective energy storage density W rec =5.86 J cm -3 , energy storage efficiency η = 86.7%.
[0009] The energy storage composite ceramic material with an internal crystalline structure of the present invention is characterized in that it is synthesized by a conventional solid phase sintering method. The specific steps include:
[0010] (1) Based on The four raw materials of BaCO3, CaCO3, TiO2 and ZrO2 were weighed respectively according to the stoichiometric ratio of the elements in the ceramic material, and the weighed raw materials were placed in a ball milling jar, and ball milled in a planetary ball mill with anhydrous ethanol as the medium for 12 hours, and then the obtained mixture was placed in an oven at 100°C for drying;
[0011] (2) grinding the dried mixture and placing it in an alumina crucible, then calcining it at 1250° C., keeping it at that temperature for 4 h, and cooling it to room temperature along with the furnace;
[0012] (3) Pour the calcined powder into a ball mill and add anhydrous ethanol for secondary ball milling for 12 h;
[0013] (4) adding a binder to the powder obtained by the secondary ball milling, granulating, sieving, and then pressing under pressure to form a ceramic green body, and heating to perform a binder removal treatment;
[0014] If a polyvinyl alcohol (PVB) binder with a mass fraction of 10 wt.% is added, the ceramic green body is pressed under a uniaxial pressure of 500 MPa for 2 minutes, and then subjected to a binder removal treatment at 650°C, kept at this temperature for 3 hours, and then cooled to room temperature with the furnace;
[0015] (5) The green body after debinding treatment was sintered at 1400°C, kept at this temperature for 4 hours, and then cooled to room temperature. The sintered ceramic sample was polished to a thickness of 0.1 mm and the sputtering area was 0.003 cm 2 Au electrodes were used and the electrical properties of the ceramic samples were tested.
[0016] Among them, the best ceramic sample composition is 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3, with a special structure of CaTiO3 second phase segregated in the grain boundary. The breakdown electric field strength E b =553.9kV / cm, maximum polarization P max =35.21μC / cm 2 , the remnant polarization P r =4.44μC / cm 2 , polarization difference △P=30.77μC / cm 2 Calculate the effective energy storage density W rec =5.86 J cm -3 , energy storage efficiency η=86.7%. It has good energy storage application potential.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] (1) The present invention can construct a new intracrystalline BCZT multiphase structure that is different from the conventional grain boundary second phase multiphase structure by controlling the CaTiO3 component content and the intracrystalline precipitation behavior.
[0019] (2) The present invention achieves the goal of maintaining a high polarization difference ΔP while enhancing E in the 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3 composite ceramic system through the design of the internal crystal structure. b , and finally obtain a high effective energy storage density W rec =5.86 J cm -3 The energy storage efficiency η is 86.7%. It can be applied to dielectric energy storage of ceramic capacitors, and further applied to dielectric energy storage of pulse ceramic capacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the XRD spectrum of the 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3 ceramic material in the specific implementation of the present invention.
[0021] Figure 2 This is a SEM image of the 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3 ceramic material in the specific implementation of the present invention, wherein the dark particles are the CaTiO3 second phase.
[0022] Figure 3 It is the PE hysteresis loop of the 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3 ceramic material near the breakdown field in the specific implementation of the present invention. DETAILED DESCRIPTION
[0023] The present invention will be described in detail below through examples. These examples are only for the purpose of illustrative description and are not intended to limit the present invention.
[0024] The present invention provides a high energy storage density ceramic material with an endocrystal structure and its preparation, characterized in that its chemical composition is 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3. The raw materials include: BaCO3, CaCO3, TiO2, and ZrO2. The specific preparation method is as follows: first, weigh the raw materials according to the stoichiometric ratio of each component, then put them into a ball mill and use anhydrous ethanol as the medium for ball milling for 12 hours, then place the resulting mixture in a 100°C oven for drying; after grinding the dried mixture, place it in a sealed alumina crucible and calcine it at 1250°C, keep it warm for 4 hours, and cool it to room temperature with the furnace; place the resulting calcined product and the ball milling medium anhydrous ethanol in a ball mill for secondary ball milling for 12 hours, then dry the ball milling slurry at 100°C; add a binder with a mass fraction of about 10wt.% to the dried powder, granulate, sieve, and press it into a ceramic blank, sinter it at 1400°C after debinding treatment, keep it warm for 4 hours, and cool it to room temperature with the furnace. The sintered ceramic sample is polished to a thickness of 0.1mm and the sputtering area is 0.003cm 2 Au electrodes were used and the electrical properties of the ceramic samples were tested.
[0025] The essential features and significant advantages of the present invention are further illustrated by the following examples. It should be noted that the present invention is by no means limited to the described examples.
[0026] Embodiment 1:
[0027] BaCO3, CaCO3, TiO2, and ZrO2 were weighed according to the chemical formula 0.9BaTiO3-0.05BaZrO3-0.05CaTiO3, and ball-milled for 12 hours using anhydrous ethanol as the medium. The mixture was dried at 100°C and calcined at 1250°C for 4 hours; anhydrous ethanol was then added for a second ball-milling for 12 hours, and a binder with a mass fraction of about 10wt.% was added to the dried powder. The powder was granulated, sieved, and pressed into a ceramic blank. After debinding treatment, it was sintered at 1400°C, kept warm for 4 hours, and cooled to room temperature with the furnace. The sintered ceramic sample was polished to a thickness of 0.1mm and the sputtering area was 0.003cm 2 Au electrodes were used and the electrical properties of the ceramic samples were tested.
[0028] Embodiment 2:
[0029] The preparation of 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3 ceramic material is the same as in Example 1.
[0030] Embodiment 3:
[0031] The preparation of 0.21BaTiO3-0.395BaZrO3-0.395CaTiO3 ceramic material is the same as in Example 1.
[0032] Table 1 Performance comparison of the above embodiments
[0033]
Claims
1. A high energy storage density composite ceramic material with an internal crystalline structure, characterized in that: The matrix chemical composition of the ceramic material is: The value of x is 0.21 to 0.90; the preferred internal crystalline structure is x=0.65, i.e. 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3.
2. A high energy storage density composite ceramic material with an endogenous crystalline structure according to claim 1, characterized in that: The chemical composition of the matrix is 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3, and it has a special structure in which the CaTiO3 second phase is segregated within the grain boundaries.
3. A high energy storage density composite ceramic material with an endogenous crystalline structure according to claim 1, characterized in that: The chemical composition of the matrix is 0.65BaTiO3-0.175BaZrO3-0.175CaTiO3, and its effective energy storage density is W rec =5.86Jcm -3 , energy storage efficiency η = 86.7%.
4. A method for preparing a high energy storage density multiphase ceramic material having an internal crystalline structure according to claims 1-3, characterized in that: The preparation is carried out by the traditional solid phase method, which specifically includes the following steps: (1) According to the chemical formula The molar ratio of each element in the raw materials BaCO3, CaCO3, ZrO2, TiO2 is weighed, wherein the value of x is 0.21 to 0.90, and the preferred internal crystal structure x=0.65; (2) The weighed raw materials are placed in a ball mill, and ball milled in anhydrous ethanol as a medium, and then dried. The dried powder is calcined at 1250° C. for 4 h and cooled in the furnace; (3) subjecting the cooled powder from step (2) to secondary ball milling and drying, and grinding and granulating the dried powder; (4) After the powder obtained by granulation in step (3) is allowed to stand, it is pressed into a green body, which is then subjected to a binder removal treatment, and finally sintered at 1400° C., kept at that temperature for 4 h, and cooled to room temperature with the furnace to obtain the target material.
5. The method according to claim 4, characterized in that Step (3) uses PVB granulation, and step (4) debinding the green body at 650°C.
6. Application of the high energy storage density multiphase ceramic material with an internal crystalline structure as described in claims 1-3 for energy storage in energy storage ceramic capacitors, and further for dielectric energy storage in pulse ceramic capacitors.
Citation Information
Patent Citations
Lead-free piezoelectric ceramic material with high transduction coefficient and preparation method thereof
CN113582682A
Dielectric ceramic material with high energy storage performance and negative capacitance temperature coefficient and preparation
CN116120058A
JP1973058010A
Dielectric ceramic compositions of BaTiO{HD 3{B -BaZrO{HD 3{B -CaTiO{HD 3 {B system
US3969252A