High-density REBCO single-phase superconducting target material and preparation method thereof

By using a co-precipitation method of lanthanide metals, barium compounds, and copper compounds, along with spark plasma sintering, the problems of low density and carbon contamination in REBCO targets were solved, enabling the preparation of high-density REBCO targets and improving coating quality.

CN118930225APending Publication Date: 2024-11-12SUZHOU ZHICAI TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411049754.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing REBCO target preparation methods are difficult to achieve high density, resulting in poor coating quality. Furthermore, atmospheric pressure sintering is prone to introducing carbon contamination, and spark plasma sintering time is relatively short.

Method used

A high-density REBCO single-phase superconducting target was prepared by co-precipitation of lanthanide metals, barium compounds, and copper compounds after dissolution, combined with pH adjustment with oxalic acid, ball milling, and spark plasma sintering. The raw material ratio and process parameters were controlled to obtain high-purity precursor powder, and high density was achieved by spark plasma sintering.

Benefits of technology

A high-density REBCO single-phase superconducting target with a relative density of over 99% was prepared, avoiding carbon pollution and improving coating quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930225A_ABST
    Figure CN118930225A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a high-density REBCO single-phase superconducting target material and a preparation method thereof. The method comprises the following steps: S1, respectively dissolving a lanthanide metal compound, a barium compound and a copper compound in an acid solution to obtain a lanthanide metal solution, a barium solution and a copper solution; mixing the lanthanide metal solution, the barium solution and the copper solution to obtain a mixed solution; the molar ratio of lanthanide metal to barium to copper in the mixed solution is 1: 2: 3; s2, excessive oxalic acid is added into the mixed solution, and then the pH of the mixed solution is adjusted to 5 with ammonia water; s3, the mixed solution is heated and aged, and precipitates are generated in the mixed solution; s4, washing and drying the precipitate to obtain precursor powder; s5, calcining the precursor powder to obtain REBCO single-phase nano powder; s6, the REBCO single-phase nano powder is subjected to ball milling treatment; s7, performing compression molding on the ball-milled REBCO powder to obtain an REBCO biscuit; and S8, the REBCO biscuit is subjected to spark plasma sintering, and the high-density REBCO single-phase superconducting target material is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superconducting materials, and in particular relates to a high-density REBCO single-phase superconducting target material and a preparation method thereof. Background Art

[0002] Superconducting materials have macroscopic quantum phenomena such as zero resistance and complete anti-magnetism that conventional materials do not have. The use of superconducting materials can realize many disruptive technologies such as super-strong magnetic fields and large-capacity energy storage that conventional technologies cannot achieve. Usually, the superconducting critical transition temperature can be used to divide existing practical superconducting materials into two categories: low-temperature superconducting materials and high-temperature superconducting materials. REBa2Cu3O7 (abbreviated as REBCO, where RE represents rare earth elements) is the second generation of high-temperature superconducting tape after Bi-based high-temperature superconductors. It is developed through thin film epitaxy and biaxial texturing technology on flexible metal substrates, which solves the problems of weak grain boundary connection and difficult mechanical processing of ceramic copper-oxygen high-temperature superconductors. It is a practical high-temperature superconducting material with relatively superior electromagnetic properties under current liquid nitrogen temperature operation. The REBCO superconducting layer in the current commercial high-temperature superconducting tape is mainly prepared by sputtering deposition of REBCO targets.

[0003] At present, the main methods for preparing REBCO targets are hot pressing sintering, pressureless sintering, spark plasma sintering, etc. Patent CN114105631A uses the pressureless sintering method to prepare superconducting targets with a density of 4.8 to 6.3 g / cm 3 , but the superconducting phase accounts for only 85%; the density of the rare earth barium copper oxide superconducting target prepared by non-vacuum pressure sintering in patent CN111943674B is only 85%; the density of the europium barium copper oxide superconducting target prepared by normal pressure sintering in patent CN116606131A is less than 95%; the density of the YBCO target prepared by spark plasma sintering of powder prepared by solid phase method in patent CN116023127A is only 95%.

[0004] Density is a key performance indicator of target materials that affects coating quality, and improving target density is one of the basic means to improve coating quality. Although hot pressing sintering can effectively improve target density, the long sintering time is prone to introduce carbon contamination. Although normal pressure sintering can avoid carbon contamination, the density of the sintered body is often not ideal. Spark plasma sintering has a shorter time, carbon contamination can be almost avoided, and a higher density can be achieved. Summary of the invention

[0005] In view of this, on the one hand, some embodiments disclose a method for preparing a high-density REBCO single-phase superconducting target material, comprising the steps of:

[0006] S1, a lanthanide metal compound, a barium compound, and a copper compound are dissolved in an acid solution to obtain a lanthanide metal solution, a barium solution, and a copper solution; the lanthanide metal solution, the barium solution, and the copper solution are mixed to obtain a mixed solution; the molar ratio of the lanthanide metal, barium, and copper in the mixed solution is 1:2:3;

[0007] S2, adding excess oxalic acid to the mixed solution, and then adjusting the pH of the mixed solution to 5 with ammonia water;

[0008] S3, the mixed solution is heated and aged, and a precipitate is generated in the mixed solution;

[0009] S4, the precipitate is washed and dried to obtain a precursor powder;

[0010] S5, the precursor powder is calcined to obtain REBCO single-phase nanopowder;

[0011] S6, REBCO single-phase nanopowder after ball milling;

[0012] S7, pressing the ball-milled REBCO powder into a REBCO green body;

[0013] S8, REBCO green billet is subjected to spark plasma sintering to obtain high-density REBCO single-phase superconducting target.

[0014] Furthermore, in some embodiments of the method for preparing a high-density REBCO single-phase superconducting target material, in step S1, the acid solution is a combination of one or more of hydrochloric acid, nitric acid or sulfuric acid.

[0015] Some embodiments disclose a method for preparing a high-density REBCO single-phase superconducting target material. In step S1, the lanthanide metal compound is a combination of one or more oxides or chlorides of light rare earth elements such as lanthanum, cerium, praseodymium, and neodymium, or heavy rare earth elements such as terbium, dysprosium, and holmium; the barium compound is barium oxide or barium chloride; and the copper compound is copper oxide or copper chloride.

[0016] In the method for preparing a high-density REBCO single-phase superconducting target material disclosed in some embodiments, in step S3, the mixed solution is aged at 70 to 90° C. for 8 to 15 hours.

[0017] In the method for preparing a high-density REBCO single-phase superconducting target material disclosed in some embodiments, in step S4, the precipitate is washed in deionized water and alcohol in sequence, and then dried at 80-100°C.

[0018] In the method for preparing a high-density REBCO single-phase superconducting target material disclosed in some embodiments, in step S5, calcination is performed in an oxygen atmosphere, the calcination temperature is 900-1200° C., and the oxygen flow rate ranges from 5-15 sccm.

[0019] In the method for preparing a high-density REBCO single-phase superconducting target material disclosed in some embodiments, in step S6, the ball milling speed is set to 240-300 rpm.

[0020] In the method for preparing a high-density REBCO single-phase superconducting target material disclosed in some embodiments, in step S8, the spark plasma sintering temperature is set to 800-1000° C., the pressure is set to 15-50 MPa, and the current is set to 100-2000A.

[0021] On the other hand, some embodiments disclose a high-density REBCO single-phase superconducting target material obtained by a method for preparing a high-density REBCO single-phase superconducting target material.

[0022] Furthermore, some embodiments disclose a high-density REBCO single-phase superconducting target material, in which the target material contains only a single-phase superconducting phase REBa2Cu3O7, and the relative density is more than 99%.

[0023] The method for preparing a high-density REBCO single-phase superconducting target disclosed in an embodiment of the present invention uses a lanthanide metal compound, a barium compound and a copper compound to prepare a high-density REBCO single-phase superconducting target. By strictly controlling the ratio of raw materials and combining a solution co-precipitation method, a precursor powder with uniform mixing and uniform particle size distribution is obtained. The precursor powder is calcined to obtain a REBCO single-phase nano powder. The high-density REBCO single-phase superconducting target is further obtained through ball milling, molding and spark plasma sintering. The target contains only a single-phase superconducting phase REBa2Cu3O7, and the relative density is more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the XRD pattern of the high-density YBCO single-phase superconducting target in Example 1;

[0025] Figure 2 This is the SEM image of the high-density GdBCO single-phase superconducting target in Example 3. DETAILED DESCRIPTION

[0026] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.

[0027] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.

[0028] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values ​​clearly listed as the limits of the range, but also all independent values ​​or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values ​​of 1% to 5%, but also the independent values ​​and sub-ranges within the range shown. Therefore, independent values ​​such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.

[0029] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.

[0030] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.

[0031] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.

[0032] In some embodiments, a method for preparing a high-density REBCO single-phase superconducting target material comprises the steps of:

[0033] S1, lanthanide metal compound, barium compound, copper compound are dissolved in acid solution respectively to obtain lanthanide metal solution, barium solution and copper solution; lanthanide metal solution, barium solution and copper solution are mixed to obtain mixed solution; the molar ratio of lanthanide metal, barium and copper in the mixed solution is 1:2:3; usually, in the process of dissolving metal compound in acid solution, heating and stirring are selected to strengthen the dissolution process; strictly controlling the molar ratio of lanthanide metal, barium and copper to 1:2:3 is a necessary condition for realizing the preparation of single-phase REBCO powder and target material; lanthanide metal solution refers to an acid solution containing lanthanide metal ions; barium solution refers to an acid solution containing barium ions; copper solution refers to an acid solution containing copper ions;

[0034] S2. Add an excess of oxalic acid to the mixed solution, and then adjust the pH of the mixed solution to 5 with ammonia water. Usually, the oxalic acid solution can be added to the mixed solution in small amounts and multiple times. Then, add ammonia water to adjust the pH of the mixed solution until the pH is 5. Experimental data with a pH of 3 to 7 show that it is difficult to form a superconducting phase when the pH is too high, and it is easy to generate an impurity phase when the pH is too low. The optimal value is 5.

[0035] S3, the mixed solution is heated and aged, and a precipitate is generated in the mixed solution; aging is conducive to grain growth and impurity removal, and heating and stirring during the aging process will increase the dissolution rate of the precipitate and the diffusion rate of ions in the solution, thereby shortening the aging time;

[0036] S4. The precipitate is washed and dried to obtain a precursor powder; washing can remove impurity ions in the precursor, which helps to obtain a precursor powder with higher purity; washing with deionized water and alcohol alternately 4 to 5 times can make the precursor powder reach a stable purity;

[0037] S5. The precursor powder is calcined to obtain REBCO single-phase nano powder. The calcination is generally carried out in an oxygen atmosphere to prevent the REBCO powder from losing oxygen. The calcination temperature is generally selected to be 900-1200°C. If the calcination temperature is too high, the grains will grow, and if the calcination temperature is too low, the REBCO single-phase powder will not be formed.

[0038] S6, REBCO single-phase nano powder is ball-milled; ball-milling helps reduce powder agglomeration and improve powder activity; dry milling or alcohol medium wet milling can be used;

[0039] S7, the REBCO powder after ball milling is molded to obtain a REBCO green billet; the green billet molding pressure directly affects the subsequent sintering process, such as sintering time, sintering temperature, etc.;

[0040] S8, REBCO green billet is subjected to spark plasma sintering to obtain high-density REBCO single-phase superconducting target; spark plasma sintering can reduce the sintering time, thereby effectively reducing carbon pollution.

[0041] Usually, metal oxide or metal chloride powder is weighed according to a set ratio, dissolved and diluted with acid, then oxalic acid solution is added and adjusted to a suitable pH value with ammonia water, and heated and aged to form a precursor precipitate; the precursor precipitate is centrifugally washed and dried to obtain a precursor powder, and the dried precursor powder is calcined to generate REBCO single-phase nanopowder; the calcined REBCO powder is ball-milled and then molded or cold isostatically pressed, and a highly dense, carbon-free and single superconducting REBCO target blank is obtained through spark plasma sintering, and a finished target material is obtained through cutting, polishing and binding.

[0042] In the method for preparing a high-density REBCO single-phase superconducting target disclosed in some embodiments, in step S1, the acid solution is a combination of one or more of hydrochloric acid, nitric acid or sulfuric acid. Generally, a hydrochloric acid solution, a nitric acid solution or a sulfuric acid solution is used to dissolve the metal compound, or a combination of two or three acids can be used to dissolve the metal compound, such as a mixed acid solution composed of dilute nitric acid and dilute sulfuric acid, or a mixed acid solution composed of dilute hydrochloric acid and dilute nitric acid.

[0043] Some embodiments disclose a method for preparing a high-density REBCO single-phase superconducting target material. In step S1, the lanthanide metal compound is a combination of one or more oxides or chlorides of light rare earth elements such as lanthanum, cerium, praseodymium, and neodymium, or heavy rare earth elements such as terbium, dysprosium, and holmium; the barium compound is barium oxide or barium chloride; and the copper compound is copper oxide or copper chloride. Generally, lanthanide metals are light rare earth elements such as lanthanum, cerium, praseodymium, neodymium, or heavy rare earth elements such as terbium, dysprosium, and holmium. Lanthanide metal compounds refer to compounds containing the above-mentioned lanthanide metal elements, for example, they can be lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, terbium oxide, dysprosium oxide, holmium oxide, or lanthanum chloride, cerium chloride, praseodymium chloride, neodymium chloride, terbium chloride, dysprosium chloride, and holmium chloride; as a raw material for preparing high-density REBCO single-phase superconducting target material, the lanthanide metal compound can be a compound of one of the above-mentioned lanthanide metals, or a combination of compounds of multiple lanthanide metals; barium compounds are compounds containing barium elements, such as barium oxide or barium chloride; copper compounds are compounds containing copper elements, such as copper oxide or copper chloride.

[0044] In the method for preparing a high-density REBCO single-phase superconducting target disclosed in some embodiments, in step S3, the mixed solution is aged at 70 to 90° C. for 8 to 15 hours. Generally, the heating aging process of the mixed solution can be carried out in a water bath, the water bath temperature is controlled between 70 and 90° C., and the aging time is controlled between 8 and 15 hours. Generally, during the heating aging process of the mixed solution, lanthanide metal ions, barium ions, and copper ions co-precipitate to form a uniformly mixed precipitate.

[0045] In the method for preparing a high-density REBCO single-phase superconducting target disclosed in some embodiments, in step S4, the precipitate is washed in deionized water and alcohol in sequence, and then dried at 80-100°C. Usually, the collected mixed precipitate needs to be washed to remove heteroatoms and heteroions therein, which is conducive to finally obtaining a high-density single-phase superconducting target; usually, it can be washed with deionized water and alcohol in sequence for multiple times until impurities are completely removed; the washed precipitate is further dried to obtain a precursor powder; usually, the drying is performed in an oven at 80-100°C.

[0046] In the method for preparing a high-density REBCO single-phase superconducting target material disclosed in some embodiments, in step S5, calcination is performed in an oxygen atmosphere, the calcination temperature is 900-1200° C., and the oxygen flow rate ranges from 5-15 sccm.

[0047] In the method for preparing a high-density REBCO single-phase superconducting target disclosed in some embodiments, in step S6, the ball milling speed is set to 240-300 rpm. Generally, dry milling or alcohol medium wet milling can be used, and the ball milling speed is generally set to 240-300 rpm.

[0048] Some embodiments disclose a method for preparing a high-density REBCO single-phase superconducting target material. In step S7, the ball-milled REBCO powder is molded to obtain a REBCO blank. Usually, molding or cold isostatic pressing can be selected, or a molding method of first molding and then cold isostatic pressing can be selected, wherein the molding pressure can be selected to be 5 to 10 MPa, and the cold isostatic pressing pressure can be selected to be 50 to 200 MPa.

[0049] In the method for preparing a high-density REBCO single-phase superconducting target material disclosed in some embodiments, in step S8, the spark plasma sintering temperature is set to 800-1000° C., the pressure is set to 15-50 MPa, and the current is set to 100-2000A.

[0050] On the other hand, some embodiments disclose a high-density REBCO single-phase superconducting target material obtained by a method for preparing a high-density REBCO single-phase superconducting target material.

[0051] Furthermore, some embodiments disclose a high-density REBCO single-phase superconducting target material, in which the target material contains only a single-phase superconducting phase REBa2Cu3O7, and the relative density is more than 99%.

[0052] The technical details are further illustrated below in conjunction with embodiments.

[0053] Example 1

[0054] In Example 1, the method for preparing a high-density YBCO single-phase superconducting target material includes:

[0055] S1, yttrium oxide, barium oxide, and copper oxide powders are dissolved in a hydrochloric acid solution to obtain yttrium chloride solution, barium chloride solution, and copper chloride solution; the yttrium chloride solution, barium chloride solution, and copper chloride solution are mixed to obtain a mixed solution; the molar ratio of lanthanide metal, barium, and copper in the mixed solution is 1:2:3;

[0056] S2. Add an excess of oxalic acid to the mixed solution and stir it, then add ammonia water dropwise to adjust the pH of the mixed solution to 5, and continue stirring for half an hour;

[0057] S3, the mixed solution is heated to 80°C in a water bath for aging, and the aging is continued for 10 hours to generate a precipitate;

[0058] S4, the precipitate was washed four times with deionized water and alcohol, and then dried in a drying oven at 80°C to obtain a precursor powder;

[0059] S5, the precursor powder was calcined at 950°C and 10 sccm oxygen flow for 10 h to obtain YBCO single-phase nanopowder;

[0060] S6, YBCO single-phase nano powder was ball-milled; the ball-milling speed was 280 rpm, the ball-to-material ratio was 3:1, and the ball-milling time was 8 h;

[0061] S7, the YBCO powder after ball milling is molded under a pressure of 8 MPa, and then subjected to cold isostatic pressing at 150 MPa to obtain a YBCO green billet;

[0062] S8, YBCO green billet is placed in a high-temperature steel mold for spark plasma sintering, the sintering temperature is 840 ° C, the sintering time is 15 min, the current is 1000 A, and the pressure is 40 MPa to obtain a high-density YBCO single-phase superconducting target.

[0063] The blocks after spark plasma sintering are polished and bound to obtain a YBCO single-phase target with a density of 99.4%.

[0064] Example 2

[0065] In Example 2, the method for preparing a high-density EBCO single-phase superconducting target material includes:

[0066] S1, 12g of erbium oxide, 24g of barium oxide, and 18.7g of copper oxide powder are dissolved in a mixture of dilute nitric acid and dilute sulfuric acid to obtain an erbium solution, a barium solution, and a copper solution; the erbium solution, the barium solution, and the copper solution are mixed to obtain a mixed solution;

[0067] S2. Add 10% excess oxalic acid to the mixed solution and stir, then add ammonia water dropwise to adjust the pH of the mixed solution to 5, and continue stirring for half an hour;

[0068] S3, the mixed solution is heated to 85°C in a water bath for aging, and the aging is continued for 10 hours to generate a precipitate;

[0069] S4, the precipitate is washed repeatedly with deionized water and alcohol for 4-5 times, and then dried in a drying oven at 85°C to obtain a precursor powder;

[0070] S5, the precursor powder was calcined at 1100°C and 10 sccm oxygen flow for 12 h to obtain EBCO single-phase nanopowder;

[0071] S6, EBCO single-phase nanopowder was ball-milled with alcohol; the ball-milling speed was 280 rpm, the ball-to-material ratio was 3:1, and the ball-milling time was 8 h; after ball-milling, it was dried at 80 °C for 6 h;

[0072] S7, the ball-milled EBCO powder is molded under a pressure of 10 MPa to obtain an EBCO green billet;

[0073] S8. The EBCO green billet is placed in a graphite mold for spark plasma sintering at a sintering temperature of 950°C, a sintering time of 15 min, a current of 1000 A, and a pressure of 50 MPa to obtain a highly dense EBCO single-phase superconducting target.

[0074] The block after spark plasma sintering can be polished and bound to obtain an EBCO single-phase target with a density of 99.2%.

[0075] Example 3

[0076] In Example 3, the method for preparing a high-density GdBCO single-phase superconducting target material includes:

[0077] S1, 20g of gadolinium oxide, 31.6g of barium oxide, and 22.8g of copper oxide powder are dissolved in a hydrochloric acid solution to obtain a gadolinium solution, a barium solution, and a copper solution; the gadolinium solution, the barium solution, and the copper solution are mixed to obtain a mixed solution;

[0078] S2, adding oxalic acid to the mixed solution and stirring, then adding ammonia water dropwise to adjust the pH of the mixed solution to 5, and continuing stirring for half an hour;

[0079] S3, the mixed solution is heated to 90°C in a water bath for aging, and the aging is continued for 9 hours to generate a precipitate;

[0080] S4, the precipitate was washed with deionized water and alcohol four times in sequence, and then dried in a drying oven at 100°C for 6 hours to obtain a precursor powder;

[0081] S5, the precursor powder was calcined at 1050°C and 15 sccm oxygen flow for 10 h to obtain GdBCO single-phase nanopowder;

[0082] S6 and GdBCO single-phase nanopowders were subjected to ball milling treatment; the ball milling speed was 260 rpm, the ball-to-material ratio was 3:1, and the ball milling time was 6 h;

[0083] S7, the ball-milled GdBCO powder is cold isostatically pressed under a pressure of 18 MPa to obtain a G-point BCO green billet;

[0084] S8, EBCO green billet is subjected to spark plasma sintering at a sintering temperature of 920°C, a sintering time of 10 min, a current of 1000 A, and a pressure of 30 MPa to obtain a highly dense GdBCO single-phase superconducting target.

[0085] The block after spark plasma sintering can be polished and bound to obtain a GdBCO single-phase target with a density of 99.5%.

[0086] The method for preparing a high-density REBCO single-phase superconducting target disclosed in an embodiment of the present invention uses a lanthanide metal compound, a barium compound and a copper compound to prepare a high-density REBCO single-phase superconducting target. By strictly controlling the ratio of raw materials and combining a solution co-precipitation method, a precursor powder with uniform mixing and uniform particle size distribution is obtained. The precursor powder is calcined to obtain a REBCO single-phase nano powder. The high-density REBCO single-phase superconducting target is further obtained through ball milling, molding and spark plasma sintering. The target contains only a single-phase superconducting phase REBa2Cu3O7, and the relative density is more than 99%.

[0087] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a high-density REBCO single-phase superconducting target material, characterized in that: Includes steps: S1, a lanthanide metal compound, a barium compound, and a copper compound are dissolved in an acid solution to obtain a lanthanide metal solution, a barium solution, and a copper solution; the lanthanide metal solution, the barium solution, and the copper solution are mixed to obtain a mixed solution; the molar ratio of the lanthanide metal, barium, and copper in the mixed solution is 1:2:3; S2, adding excess oxalic acid to the mixed solution, and then adjusting the pH of the mixed solution to 5 with ammonia water; S3, the mixed solution is heated and aged, and a precipitate is generated in the mixed solution; S4, the precipitate is washed and dried to obtain a precursor powder; S5, the precursor powder is calcined to obtain REBCO single-phase nanopowder; S6, REBCO single-phase nanopowder after ball milling; S7, pressing the ball-milled REBCO powder into a REBCO green body; S8, REBCO green billet is subjected to spark plasma sintering to obtain high-density REBCO single-phase superconducting target.

2. The method for preparing a high-density REBCO single-phase superconducting target material according to claim 1, characterized in that: In step S1, the acid solution is a combination of one or more of hydrochloric acid, nitric acid or sulfuric acid.

3. The method for preparing a high-density REBCO single-phase superconducting target material according to claim 1, characterized in that: In step S1, the lanthanide metal compound is a combination of one or more oxides or chlorides of light rare earth elements such as lanthanum, cerium, praseodymium, and neodymium, or heavy rare earth elements such as terbium, dysprosium, and holmium; the barium compound is barium oxide or barium chloride; and the copper compound is copper oxide or copper chloride.

4. The method for preparing a high-density REBCO single-phase superconducting target material according to claim 1, characterized in that: In step S3, the mixed solution is aged at 70-90° C. for 8-15 hours.

5. The method for preparing a high-density REBCO single-phase superconducting target material according to claim 1, characterized in that: In step S4, the precipitate is washed in deionized water and alcohol in sequence, and then dried at 80-100°C.

6. The method for preparing a high-density REBCO single-phase superconducting target material according to claim 1, characterized in that: In step S5, calcination is performed in an oxygen atmosphere, the calcination temperature is 900-1200° C., and the oxygen flow rate ranges from 5-15 sccm.

7. The method for preparing a high-density REBCO single-phase superconducting target material according to claim 1, characterized in that: In step S6, the ball milling speed is set to 240-300 rpm.

8. The method for preparing a high-density REBCO single-phase superconducting target material according to claim 1, characterized in that: In step S8, the spark plasma sintering temperature is set to 800-1000°C, the pressure is set to 15-50MPa, and the current is set to 100-2000A.

9. High-density REBCO single-phase superconducting target, characterized in that: The high-density REBCO single-phase superconducting target is obtained by the preparation method of any one of claims 1 to 8.

10. The high-density REBCO single-phase superconducting target material according to claim 9, characterized in that: The target material contains only single-phase superconducting phase REBa2Cu3O7, and the relative density is more than 99%.

Citation Information

Patent Citations

  • Process for producing YBCO superconducting thin film target material

    CN101492291A

  • Preparation method of lanthanide series rare earth doped indium zinc oxide nano powder

    CN116002749A

  • Target for forming superconducting thin film and method for producing the same

    JP2013163847A

  • Coprecipitation process for preparing raw material powder for y1ba2cu3ox oxide superconductor

    US5122508A

Cited By

  • High-density superconducting doped rare earth barium copper oxide and preparation method and application thereof

    CN119874349A

  • Method for preparing Nb3Sn superconducting strip based on ligand assistance

    CN120913949A

  • Preparation method of nanoscale high-purity superconducting powder

    CN122531881A