Ultralow dielectric loss microwave dielectric high-entropy ceramic material and preparation method thereof
Through the preparation method of high-entropy ceramic material (Nd0.2Eu0.2Y0.2Ho0.2) VO4, the problem of high dielectric loss of existing microwave dielectric ceramic materials is solved, and ultra-low dielectric material with high quality factor and temperature stability is achieved. Electrical loss microwave dielectric ceramic materials, suitable for a variety of microwave devices.
Patent Information
- Application Number
- CN202410765609.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-11
AI Technical Summary
When existing microwave dielectric ceramic materials meet the requirements of dielectric properties, the dielectric loss is high, and it is difficult to meet the high-performance requirements of dielectric constant, quality factor and resonant frequency temperature coefficient at the same time. There is a lack of theoretical prediction of microstructure and dielectric properties. relation.
The preparation method of high-entropy ceramic material (Nd0.2Eu0.2Y0.2Ho0.2) VO4 is adopted, by mixing oxide powder with a purity higher than 99.9% according to a specific molar ratio, wet grinding, pre-sintering and sintering, and adding polyvinyl alcohol The solution is used as a binder to prepare microwave dielectric high-entropy ceramic materials with ultra-low dielectric loss.
It achieves a quality factor Q×f value that is more than 2 times higher than traditional materials and good temperature stability. The dielectric constant is between 11.36 and 11.55. It is suitable for microwave devices such as antenna substrates, resonators and filters.
Smart Images

Figure CN118754658A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic materials, and in particular to an ultra-low dielectric loss microwave dielectric high entropy ceramic material and a preparation method thereof. Background Art
[0002] Microwave dielectric ceramics refer to new electronic ceramics that are used as dielectric materials in microwave frequency bands (mainly UHF and SHF bands) circuits and perform one or more functions. They are widely used as components such as resonators, filters, dielectric substrates and dielectric waveguide circuits in modern communications. They are key basic materials for modern communication technology and have been used in portable mobile phones, car phones, cordless phones, TV satellite receivers and military radars. They are playing an increasingly important role in the miniaturization and integration of modern communication tools. "High entropy" is a new material design theory that has emerged in recent years. It has become a hot topic in the field of material research. Its concept was originally developed from high entropy alloys (HEAs). The world of high entropy materials is diverse. By adding component elements, some novel properties appear in the materials. Then, by adjusting the concentration of the components to fine-tune their performance, a large number of excellent properties of the materials can be discovered. Compared with traditional ceramic materials, high entropy ceramics (HECs) have good structural stability, excellent mechanical properties and excellent electrical properties, and are expected to be used in electronics, energy and environment.
[0003] The concept of high entropy effect comes from high entropy alloys, and the concept of high entropy alloys was first proposed and determined by two research groups from National Tsing Hua University in Taiwan, China and Bradford University in the UK. So far, it has gone through 15 years of development. At least 5 alloying elements are selected from metals such as Cu, Co, Ni, Cr, Al, Fe and V, mixed in a nearly equimolar ratio, and prepared by sputtering, melting, casting and other methods. The alloy or alloy coating has a simple single-phase face-centered cubic or body-centered cubic crystal structure and extraordinary mechanical properties, and has phase stability that conventional metals do not have. Defining this alloy as a high entropy alloy opened the prelude to the study of high entropy alloys. With the continuous deepening of research, the concept of high entropy has gradually expanded to other materials, such as high entropy glass, high entropy ceramics, high entropy thermoelectric materials, high entropy polymers, etc., and some properties of these high entropy materials have also been improved to a certain extent. The study of high entropy ceramics can be traced back to 2015, when Rosta and Maria from North Carolina State University in the United States and Curtarolo from Duke University first reported a rock salt structure entropy-stabilized oxide ceramic, namely high entropy ceramics. Subsequently, more and more high-entropy ceramics, including high-entropy oxide ceramics with fluorite structure, perovskite structure, and spinel structure, as well as non-oxide high-entropy ceramics such as borides, carbides, nitrides, silicides, and sulfides, have emerged like mushrooms after a rain and gradually become a hot topic.
[0004] Dielectric ceramics used in microwave frequency bands should meet the following dielectric property requirements: (1) Serial dielectric constant ε r To meet the requirements of different frequencies and different applications; (2) High quality factor Q value or low dielectric loss tanδ to reduce noise, generally requiring Q×f ≥ 10000GHz; (3) Temperature coefficient of resonant frequency τ f As small as possible to ensure that the device has good thermal stability, generally requiring -10ppm / ℃≤τ f ≤+10ppm / ℃. After decades of research and exploration, domestic and foreign scholars have developed a large number of microwave dielectric materials. The number of microwave properties of microwave dielectric ceramic systems published in global public journals has reached thousands. Now, according to the size of the dielectric constant of microwave dielectric materials and the different application frequency ranges, all microwave dielectric ceramics are divided into four categories: high, medium, low, and ultra-low microwave dielectric ceramic materials:
[0005] (1) High dielectric constant microwave dielectric ceramics mainly refer to those with a dielectric constant greater than 60. At present, the developed high dielectric constant ceramics are mainly composed of tungsten bronze BaO-Ln2O3-TiO2 series, composite perovskite CaO-Li2O-Ln2O3-TiO2 series, lead-based perovskite series, etc. This type of material not only has a high dielectric constant, but also has a common structural feature that there are oxygen octahedral structural units with common vertices between the material crystals. It is mainly used as microwave dielectric resonator in communication equipment.
[0006] (2) Dielectric constant microwave dielectric ceramics mainly refer to those with a dielectric constant between 35 and 60, a quality factor greater than 20000 GHz, and a resonant frequency temperature coefficient between -10 ppm / ℃ and 10 ppm / ℃. This type of microwave dielectric ceramics is mainly composed of Ba-based composite perovskite Ba(B' 1 / 3 B" 2 / 3 )O3 (B'=Zn, Co, Mg, Mn, Ni; B"=Nb, Ta) ceramics are the most common. In addition, BaO-TiO2 system, (Zr, Sn)TiO4 system, Ln2O3-TiO2 system, etc. are also the main systems in intermediate microwave dielectric ceramics. Since the frequency f of this type of ceramic is between 4 and 8 GHz, it is mainly used in military radars, satellite communications, and mobile communication base stations.
[0007] (3) Low dielectric constant microwave dielectric ceramics mainly refer to those with a dielectric constant between 15 and 35, a quality factor greater than 50,000 GHz, and a resonant frequency temperature coefficient between -5 ppm / °C and 5 ppm / °C. They mainly include Al2O3, MgAl2O4, and composite perovskite compounds. This series of materials is widely used in the manufacture of microwave substrates, high-end microwave components, etc. because of their near-zero resonant frequency temperature coefficient and high quality factor.
[0008] (4) Ultra-low dielectric constant microwave dielectric ceramics mainly refer to those with a dielectric constant less than 15, mainly Al2O3-TiO2, Bi2O3-MoO3, Li2O-Bi2O3-MoO3, Na2O-MoO3 and other systems. They are mainly used for microwave substrates and high-end microwave components.
[0009] Due to the three performance indicators of microwave dielectric ceramics (ε r With Q×f and τ f ) are mutually constrained (see the literature: The constraining relationship between the dielectric properties of microwave dielectric ceramic materials, Zhu Jianhua, Liang Fei, Wang Xiaohong, Lv Wenzhong, Electronic Components and Materials, Issue 3, March 2005), and there are very few microwave dielectric ceramics that meet all three performance requirements. At present, most of the research on microwave dielectric ceramics is based on empirical summaries obtained through a large number of experiments, but there is no complete theory to explain the relationship between microstructure and dielectric properties. Therefore, it is theoretically impossible to predict the microwave dielectric properties of a compound from its composition and structure. Exploring and developing high-performance and low dielectric loss microwave dielectric ceramics has always been the research focus of technicians in this field. Summary of the invention
[0010] The purpose of the present invention is to provide an ultra-low dielectric loss microwave dielectric high entropy ceramic material and a preparation method thereof, aiming to provide an ultra-low dielectric loss microwave dielectric high entropy ceramic material with a higher Q×f value than traditional materials and a simpler and easier to implement preparation method.
[0011] To achieve the above object, the present invention provides an ultra-low dielectric loss microwave dielectric high entropy ceramic material, the chemical composition of the ultra-low dielectric loss microwave dielectric high entropy ceramic material is (Nd 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 )VO4.
[0012] The present invention also proposes a method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material, which is used to prepare the ultra-low dielectric loss microwave dielectric high entropy ceramic material, comprising the following steps:
[0013] Step 1: The original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 with purity >99.9% were prepared by 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 ) The composition of VO4 is weighed and mixed, wherein the molar ratio of Nd2O3, Eu2O3, Y2O3, Ho2O3 and Yb2O3 is 1:1:1:1:1;
[0014] Step 2: The raw powders in step 1 are mixed and wet-milled, dried, and pre-sintered at 900° C. in an atmosphere for 5 to 8 hours to obtain pre-sintered powders;
[0015] Step 3: Add a binder to the pre-sintered powder and granulate it, then press it into shape, and finally sinter it in an atmosphere at 1020-1060° C. for 3-6 hours to obtain the ultra-low dielectric loss microwave dielectric high entropy ceramic material.
[0016] Preferably, the binder is a polyvinyl alcohol solution with a mass concentration of 5%.
[0017] Preferably, the added mass of the binder accounts for 3% of the total mass of the original powder.
[0018] Preferably, in step 2, the process of mixing the original powders and performing wet grinding treatment is specifically to place the original powders into a wet ball mill for wet grinding treatment for 6 to 10 hours, and the ball milling medium is anhydrous ethanol.
[0019] The present invention provides an ultra-low dielectric loss microwave dielectric high entropy ceramic material and a preparation method thereof, specifically, the original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 are weighed and wet-grinded according to a ratio, dried and pre-sintered to obtain a pre-sintered powder, and then a binder is added and granulated, and the ultra-low dielectric loss microwave dielectric high entropy ceramic material is sintered after pressing and molding. It has been verified that the ultra-low dielectric loss microwave dielectric high entropy ceramic material prepared by the present invention has a resonant frequency temperature coefficient τ f The dielectric constant is as low as 11.36 to 11.55, and the quality factor Q×f is as high as 67700-76320GHz, which is more than twice the Q×f value of traditional materials (<30000GHz). It can be widely used in the manufacture of various microwave devices such as dielectric antenna substrates, resonators and filters. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 It is a schematic flow chart of the steps of a method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material of the present invention. DETAILED DESCRIPTION
[0022] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0023] The present invention proposes an ultra-low dielectric loss microwave dielectric high entropy ceramic material, the chemical composition of the ultra-low dielectric loss microwave dielectric high entropy ceramic material is (Nd 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 )VO4.
[0024] For further information, see Figure 1 The present invention also proposes a method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material, which is used to prepare the ultra-low dielectric loss microwave dielectric high entropy ceramic material, comprising the following steps:
[0025] S1: The original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 with purity > 99.9% were prepared by 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 ) The composition of VO4 is weighed and mixed, wherein the molar ratio of Nd2O3, Eu2O3, Y2O3, Ho2O3 and Yb2O3 is 1:1:1:1:1;
[0026] S2: mixing the raw powders in step S1 and wet-grinding them, drying them, and pre-sintering them in an atmosphere at 900° C. for 5 to 8 hours to obtain pre-sintered powders;
[0027] S3: adding a binder to the pre-sintered powder and granulating it, then pressing it into shape, and finally sintering it in an atmosphere at 1020-1060° C. for 3-6 hours to obtain the ultra-low dielectric loss microwave dielectric high entropy ceramic material.
[0028] The binder is a polyvinyl alcohol solution with a mass concentration of 5%.
[0029] The added mass of the binder accounts for 3% of the total mass of the original powder.
[0030] The process of mixing the original powders and performing wet grinding in step S2 specifically includes placing the original powders in a wet ball mill for wet grinding for 6 to 10 hours, and the ball milling medium is anhydrous ethanol.
[0031] As we all know, the minimization of Gibbs free energy determines the thermodynamic stability of the material. Gibbs free energy is the product of enthalpy (H) minus thermodynamic temperature (T) and entropy (S), that is, G = H-TS; so high-entropy materials with large S values are more stable. The high-entropy effect plays an important role in the formation and stabilization of high-entropy phases. Due to the high mixing entropy, the Gibbs free energy of the system is reduced, the ordering and segregation of high-entropy components are suppressed, the phase formation and stabilization of single-phase solid solutions are promoted, and the dielectric loss of microwave dielectric ceramics is reduced.
[0032] Furthermore, the present invention is further described by four specific embodiments:
[0033] Example 1
[0034] A method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material, comprising the steps of:
[0035] (1) The original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 with purity > 99.9% were prepared by 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 ) The composition of VO4 is weighed and mixed, wherein the molar ratio of Nd2O3, Eu2O3, Y2O3, Ho2O3 and Yb2O3 is 1:1:1:1:1;
[0036] (2) the raw materials in step (1) were wet ball-milled for 8 hours using anhydrous ethanol as the ball-milling medium, and then dried and pre-calcined in an atmosphere at 900° C. for 6 hours;
[0037] (3) Adding a binder to the powder obtained in step (2), granulating the powder, pressing the powder into a shape, and finally sintering the powder at 1020° C. in an atmosphere for 4 hours; the binder is a polyvinyl alcohol solution with a mass concentration of 5%, and the amount of polyvinyl alcohol added is 3% of the total mass of the powder.
[0038] Example 2
[0039] A method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material, comprising the steps of:
[0040] (1) The original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 with purity > 99.9% were prepared by 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 ) The composition of VO4 is weighed and mixed, wherein the molar ratio of Nd2O3, Eu2O3, Y2O3, Ho2O3 and Yb2O3 is 1:1:1:1:1;
[0041] (2) the raw materials in step (1) were wet ball-milled for 8 hours using anhydrous ethanol as the ball-milling medium, and then dried and pre-calcined in an atmosphere at 900° C. for 6 hours;
[0042] (3) Adding a binder to the powder obtained in step (2), granulating the powder, pressing the powder into a shape, and finally sintering the powder at 1040° C. in an atmosphere for 4 hours; the binder is a polyvinyl alcohol solution with a mass concentration of 5%, and the amount of polyvinyl alcohol added is 3% of the total mass of the powder.
[0043] Example 3
[0044] A method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material, comprising the steps of:
[0045] (1) The original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 with purity > 99.9% were prepared by 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 ) The composition of VO4 is weighed and mixed, wherein the molar ratio of Nd2O3, Eu2O3, Y2O3, Ho2O3 and Yb2O3 is 1:1:1:1:1;
[0046] (2) the raw materials in step (1) were wet ball-milled for 8 hours using anhydrous ethanol as the ball-milling medium, and then dried and pre-calcined in an atmosphere at 900° C. for 6 hours;
[0047] (3) Adding a binder to the powder obtained in step (2), granulating the powder, pressing the powder into a shape, and finally sintering the powder at 1050° C. in an atmosphere for 4 hours; the binder is a polyvinyl alcohol solution with a mass concentration of 5%, and the amount of polyvinyl alcohol added is 3% of the total mass of the powder.
[0048] Example 4
[0049] A method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material, comprising the steps of:
[0050] (1) The original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 with purity > 99.9% were prepared by 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 ) The composition of VO4 is weighed and mixed, wherein the molar ratio of Nd2O3, Eu2O3, Y2O3, Ho2O3 and Yb2O3 is 1:1:1:1:1;
[0051] (2) the raw materials in step (1) were wet ball-milled for 8 hours using anhydrous ethanol as the ball-milling medium, and then dried and pre-calcined in an atmosphere at 900° C. for 6 hours;
[0052] (3) Adding a binder to the powder obtained in step (2), granulating the powder, pressing the powder into a shape, and finally sintering the powder at 1060° C. in an atmosphere for 4 hours; the binder is a polyvinyl alcohol solution with a mass concentration of 5%, and the amount of polyvinyl alcohol added is 3% of the total mass of the powder.
[0053] Furthermore, the present invention uses a cylindrical dielectric resonator method to evaluate microwave dielectric properties. Specifically, the Hakki-Coleman method is used to measure the dielectric constant of solid materials, ε r It can only be measured at one resonant frequency corresponding to the TE011 mode. In order to avoid the problem of conduction and radiation losses, the Q value of the microwave dielectric ceramic sample can be measured by the resonant cavity method. The sample is placed in a low-loss spacer cavity. The resonant frequency temperature coefficient is a measure of the thermal stability of the resonator. It represents the "drift" of the resonant frequency relative to the temperature. The relationship between the resonant frequency and the temperature is: Where f0 is the initial resonant frequency, Δf is the change in resonant frequency, and ΔT is the temperature change. The results are shown in Table 1:
[0054] Table 1 Microwave dielectric properties
[0055]
[0056] It can be seen from Table 1 that the temperature coefficient of the resonant frequency of the ultra-low dielectric loss microwave dielectric high entropy ceramic material prepared by the present invention is τ f The dielectric constant of the material is small (-35.3~-37.3ppm / ℃), and the temperature stability is good; its dielectric constant reaches 11.36~11.55, and the quality factor Q×f value is as high as 67700-76320GHz, which is more than twice higher than the Q×f value of traditional materials (<30000GHz); it can be widely used in the manufacture of various dielectric antenna substrates, resonators, filters and other microwave devices. Specifically, it can be used to produce microwave components, including but not limited to microwave resonators, filters, oscillators or dielectric antennas.
[0057] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. An ultra-low dielectric loss microwave dielectric high entropy ceramic material, characterized in that: The chemical composition of the ultra-low dielectric loss microwave dielectric high entropy ceramic material is (Nd 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 )VO4.
2. A method for preparing an ultra-low dielectric loss microwave dielectric high entropy ceramic material, used to prepare the ultra-low dielectric loss microwave dielectric high entropy ceramic material as claimed in claim 1, characterized in that: The following steps are involved: Step 1: The original powders of Nd2O3, Eu2O3, Y2O3, Ho2O3, Yb2O3 and NH4VO3 with purity >99.9% were prepared by 0.2 Eu 0.2 Y 0.2 Ho 0.2 Yb 0.2 ) The composition of VO4 is weighed and mixed, wherein the molar ratio of Nd2O3, Eu2O3, Y2O3, Ho2O3 and Yb2O3 is 1:1:1:1:1; Step 2: The raw powders in step 1 are mixed and wet-milled, dried, and pre-sintered at 900° C. in an atmosphere for 5 to 8 hours to obtain pre-sintered powders; Step 3: Add a binder to the pre-sintered powder and granulate it, then press it into shape, and finally sinter it in an atmosphere at 1020-1060° C. for 3-6 hours to obtain the ultra-low dielectric loss microwave dielectric high entropy ceramic material.
3. The method for preparing the ultra-low dielectric loss microwave dielectric high entropy ceramic material according to claim 2, characterized in that: The binder is a polyvinyl alcohol solution with a mass concentration of 5%.
4. The method for preparing the ultra-low dielectric loss microwave dielectric high entropy ceramic material according to claim 3, characterized in that: The added mass of the binder accounts for 3% of the total mass of the original powder.
5. The method for preparing the ultra-low dielectric loss microwave dielectric high entropy ceramic material according to claim 4, characterized in that: The process of mixing the original powders and performing wet grinding in step 2 specifically includes placing the original powders in a wet ball mill for wet grinding for 6 to 10 hours, and the ball milling medium is anhydrous ethanol.
Citation Information
Patent Citations
Ultra-low dielectric constant microwave dielectric ceramic HoYV2O8 with high thermal stability and low loss
CN105036743A
Low-loss stable-temperature ultralow-dielectric-constant microwave dielectric ceramic NdY2V3O12
CN105060890A
Quentabasic zircon type structure high-entropy oxide ceramic and preparation method thereof
CN115947599A
Dielectric ceramic composition and stacked ceramic capacitor
CN1249286A
A-site high-entropy nanometer metal oxide with high conductivity, and preparation method thereof
US20220234908A1