Novel nuclear high-performance SiCf / SiC composite material and preparation method thereof

The Ti3SiC2 interface phase and matrix are prepared through magnetron sputtering and gas-phase RMI processes, which solves the problems of insufficient air tightness and thermal conductivity of SiCf/SiC composite materials for nuclear use, improves material performance and reduces process cycle and cost. Suitable for the preparation of large-sized structural parts.

CN118754693AActive Publication Date: 2024-10-11NORTHWESTERN POLYTECHNICAL UNIV

Patent Information

Application Number
CN202410981320.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing nuclear SiCf/SiC composite materials have poor air tightness, low thermal conductivity, PyC interface failure and internal pore problems during service, resulting in reduced mechanical properties and insufficient thermal conductivity. The traditional CVI process has a long preparation cycle and high cost. High, only suitable for thin-walled parts.

Method used

Magnetron sputtering combined with gas phase RMI process is used to prepare the Ti3SiC2 interface phase, and the Ti3SiC2 modified SiC matrix is ​​prepared through a single RMI process, replacing the traditional CVI process to achieve densification and performance improvement of SiCf/SiC composite materials.

Benefits of technology

It improves the air tightness, thermal conductivity and radiation resistance of SiCf/SiC composite materials, reduces the process cycle and cost, is suitable for the preparation of large-sized structural parts, and significantly improves the mechanical and thermophysical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754693A_ABST
    Figure CN118754693A_ABST
Patent Text Reader

Abstract

The invention discloses a novel nuclear high-performance SiCf / SiC composite material and a preparation method thereof, and relates to the technical field of composite materials. The method comprises the following steps: obtaining two-dimensional SiCf / Ti-Si-C-O fiber cloth; the SiCf / Ti3SiC2 interface phase two-dimensional fiber cloth is obtained through RMI process gas phase siliconizing; the SiCf / Ti3SiC2 interface phase two-dimensional fiber cloth is soaked in the slurry suspension liquid, and SiCf / Ti3SiC2 interface / TiC-TiO2 fiber cloth is obtained; shaping is carried out, such that a SiCf / Ti3SiC2 interface / TiC-TiO2 preform is obtained; and embedding the SiCf / Ti3SiC2 interface / TiC-TiO2 preform into AlSi alloy powder, carrying out liquid-phase siliconizing by adopting an RMI process, and carrying out heat preservation for 30-60 minutes at 1250-1450 DEG C in a vacuum furnace, so as to obtain the novel nuclear high-performance SiCf / SiC composite material. By adopting the gas phase and liquid phase combined successive siliconizing process, the problems of poor air tightness and low heat conductivity of the current nuclear SiCf / SiC composite material can be solved, the anti-irradiation amorphization and damage tolerance of the material can be further enhanced, the structural strength of the SiCf / SiC composite material in the service process of a reactor is improved, and the safety margin of reactor design is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite materials, and in particular to a novel high-performance SiC f / SiC composite material and preparation method thereof. Background Art

[0002] Silicon carbide (SiC) materials have high strength, small neutron absorption cross section, good resistance to radiation damage, excellent high-temperature chemical inertness, low activation, excellent high-temperature strength and structural stability, and have great application prospects in the extreme use environment of reactors. However, the intrinsic brittleness of SiC ceramics limits its practical application as a structural material. In this regard, continuous SiC fiber-reinforced SiC composites (SiC f / SiC) makes up for the shortcoming of low toughness of SiC ceramics, while also having excellent high-temperature mechanical properties and chemical inertness. It is considered to be one of the ideal candidate materials for the cladding structure of the next generation of advanced nuclear energy systems.

[0003] Nuclear SiC f The SiC / SiC composite material is composed of a SiC fiber preform, a PyC interface phase and a SiC matrix. The SiC fiber preform is obtained by weaving SiC fibers. 3 H 6 ) as the gas source, the PyC interface phase was deposited in the SiC fiber preform by chemical vapor infiltration (CVI). 3 SiCl, MTS) as the gas source, the SiC matrix is ​​continuously deposited into the preform using the CVI process until the sample is completely dense. f / SiC composites have a "bottleneck effect" during the CVI deposition process, that is, when the pores inside the fiber bundle are not fully deposited and filled, the deposition gas channel closes prematurely, resulting in the SiC f There are many pores inside the SiC composite material. Therefore, the SiC prepared by CVI process f / SiC composite materials generally have a porosity of 10%~13%.

[0004] Existing SiC for nuclear applications f / SiC composite materials use PyC interface phase, which is prone to irradiation amorphization during service, resulting in composite interface failure and SiC f / SiC composite materials have a sharp decline in mechanical properties; the existing nuclear SiC f Due to the intrinsic brittleness of the SiC ceramic matrix, SiC composite materials are prone to through cracks during service, which destroys the airtightness of the material and may cause leakage of radioactive substances.f / SiC composites are prepared by CVI process. However, due to the "bottleneck effect" of CVI process when depositing SiC matrix, SiC f There are generally 10 to 13% open pores in the SiC composite material. The presence of internal pores makes SiC f / SiC composite materials have greatly reduced air tightness and thermal conductivity; existing nuclear SiC f The optimization scheme of SiC composite materials generally uses the CVI process to prepare the interface phase and part of the SiC matrix to obtain porous SiC with certain mechanical strength. f / SiC composites, which are then densified by reactive melt infiltration (RMI) or PIP process, while introducing matrix modified phase. However, due to the large differences in intrinsic properties such as density, porosity and crystal growth orientation of ceramic phases prepared by different processes, SiC f There is a large residual stress inside the SiC composite material, which causes f / SiC composite materials have problems such as reduced load-bearing capacity, internal cracks caused by thermal mismatch, and reduced thermal conductivity during service. The current commercial application of nuclear SiC prepared by CVI process f / SiC composite materials have a long process cycle, high production cost, and are only suitable for the preparation of thin-walled parts.

[0005] At present, core SiC prepared by chemical vapor infiltration (CVI) process with pyrolytic carbon (PyC) as the interface phase f / SiC composites have poor air tightness, low thermal conductivity, and PyC interface failure under high-dose irradiation. Summary of the invention

[0006] In view of the shortcomings of the above background technology, the present invention provides a new type of high-performance SiC f / SiC composite material and preparation method thereof. The method adopts magnetron sputtering combined with gas phase RMI process to prepare Ti 3 SiC 2 Interface phase, compared with the currently reported Ti 3 SiC 2 Interface phase preparation process, the Ti prepared by this process 3 SiC 2 The interface phase has higher purity and good thermal stability, which ensures the structural integrity in the subsequent matrix preparation process.

[0007] The first object of the present invention is to provide a new type of high performance SiC fA method for preparing a SiC / SiC composite material, using a single reaction melt infiltration process to sequentially prepare an interface phase and a matrix phase of the composite material, comprising the following steps: The two-dimensional SiC fibers were placed in a magnetron sputtering instrument using SiC targets and TiO 2 The target material is co-sputtered to form a Ti-Si-CO interface layer on the surface of the SiC fiber to obtain a two-dimensional SiC f / Ti-Si-CO fiber cloth; Two-dimensional SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f / Ti-Si-CO fiber cloth was placed in a graphite crucible, and Si powder was placed at the bottom of the graphite crucible. The temperature was raised to 1450-1500 °C and kept for 30-60 min to obtain SiC f / Ti 3 SiC 2 Interfacial phase two-dimensional fiber cloth; Add TiC, TiO 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 Mixing reaction aids, and ball milling to obtain a slurry suspension; SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth is immersed in the slurry suspension to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Fiber cloth; SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The fiber cloth is stacked to form a layered preform, and the layered preform is axially pressed and dried to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Greenware; SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The green body is treated at 1200 ~ 1400℃ for 2~4h in an inert atmosphere or under vacuum conditions to obtain SiC f / Ti3 SiC 2 Interface / TiC-TiO 2 Prefabricated body; SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The preform is embedded in AlSi alloy powder and kept at 1250~1450℃ in a vacuum furnace for 30~60min to obtain Ti 3 SiC 2 The modified SiC matrix phase gives a new type of high-performance SiCf / SiC composite material for nuclear use.

[0008] Preferably, the dextrin solution is prepared by adding dextrin at a mass fraction of 0.1 to 1.0 wt.% into distilled water.

[0009] Preferably, the TiC, TiO 2 The mixed raw materials include TiC powder and TiO 2 powder; Among them, TiC powder and TiO 2 The powder molar ratio is 1:1~3:1; The TiC powder and TiO 2 The particle diameter of the powder is 5-8 μm.

[0010] Preferably, the TiC powder is replaced with a mixed powder of Ti powder and C powder.

[0011] Preferably, the Y 2 O 3 、Al 2 O 3 Mixed reaction aids include Y 2 O 3 Powder and Al 2 O 3 powder; Among them, Y 2 O 3 Powder and Al 2 O 3 The molar ratio of powder is 2:1~1:2; Y 2 O 3 Powder and Al 2 O 3 The particle diameter of the powder is 10-12 μm.

[0012] Preferably, TiC, TiO 2 Mix raw materials and Y 2 O 3 、Al2 O 3 The reaction aid is mixed, and the mass of the mixed powder is 30-50 wt.% of the mass of the solution.

[0013] Preferably, SiC f / Ti 3 SiC 2 The duration of immersion of the interfacial phase two-dimensional fiber cloth in the slurry suspension is 5 to 30 min; When axial pressure is applied to the layered preform, the axial pressure is 5 to 20 MPa and the pressure is maintained for 5 to 30 minutes; the temperature during drying is 110 to 125°C and the drying time is 24 to 48 hours.

[0014] Preferably, the AlSi alloy powder is replaced with Si powder, ZrSi alloy powder or YSi alloy powder.

[0015] The second object of the present invention is to provide a new type of high performance SiC f / SiC composite materials.

[0016] The third object of the present invention is to provide a high performance SiC f / Application of SiC composite materials in nuclear industry.

[0017] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a new type of high performance SiC for nuclear use f / SiC composite material and preparation method thereof, the present invention adopts RMI process to prepare Ti 3 SiC 2 The interface phase is then prepared 3 SiC 2 The idea of ​​modifying the SiC matrix is ​​to use a single RMI process to achieve the transformation from existing SiC fibers to SiC f / SiC composite material, including the preparation of interface phase and matrix. f / SiC composite interface phase modification, and then another process is selected to prepare the matrix, which ultimately leads to huge residual stress between the components of the composites prepared by different processes, affecting the SiC f The overall performance of the / SiC composite material is different. Ti was prepared by magnetron sputtering combined with gas phase RMI process. 3 SiC 2 Interface phase, compared with the currently reported Ti 3 SiC 2 Interface phase preparation process, the Ti prepared by this process 3 SiC 2The interface phase has higher purity, controllable thickness, and good thermal stability, which ensures the structural integrity in the subsequent matrix preparation process; the present invention draws on the prepreg process commonly used in resin-based composite materials to 3 SiC 2 The two-dimensional SiC fiber cloth of the interface phase is first impregnated with the RMI precursor, and then the fiber cloth with the RMI precursor slurry is laminated and shaped, and then heat-treated and pre-sintered to obtain an RMI preform with a certain structural strength, and finally liquid phase siliconization is performed to obtain the final dense SiC f / SiC composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The present invention provides a new type of high-performance SiC for nuclear use f / SiC composite material preparation process preparation flow chart; Figure 2 The dense SiC prepared by the present invention f / Ti 3 SiC 2 Interface / SiC-Ti 3 SiC 2 Physical picture of composite materials; Figure 3 New high-performance nuclear SiC prepared by the present invention f / SiC composite microstructure image. DETAILED DESCRIPTION

[0019] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.

[0020] The present invention is aimed at the core SiC prepared by the current chemical vapor infiltration (CVI) process with pyrolytic carbon (PyC) as the interface phase. f The Ti / SiC composites have poor air tightness, low thermal conductivity, and PyC interface failure under high-dose irradiation. 3 SiC 2 Interfacial phase, combined with liquid phase siliconization process to prepare ternary layered ceramic Ti 3 SiC 2 The matrix phase thus obtains dense SiC f / SiC composite materials. The gas phase and liquid phase combined successive siliconization process can solve the current nuclear SiC f The poor air tightness and low thermal conductivity of SiC composite materials can be further enhanced to improve the material's radiation resistance to amorphization and damage tolerance, thereby improving the SiC f / The structural strength of SiC composite materials during reactor service improves the safety margin of reactor design.

[0021] The purpose of this invention is to change the traditional nuclear SiC f CVI preparation process of / SiC composite materials, using RMI process to prepare Ti by vapor phase siliconization 3 SiC 2 Interface phase, liquid phase siliconization to prepare Ti 3 SiC 2 Modify the SiC matrix and finally obtain high-density SiC f / SiC composite materials. Among them, Ti 3 SiC 2 The interface phase replaces the PyC interface phase and greatly improves the radiation resistance of the interface phase. 3 SiC 2 Introducing into the SiC matrix can further improve the SiC f / SiC composite material damage tolerance. At the same time, SiC prepared by RMI process f The increase in density of SiC composite materials has a great effect on improving the thermal conductivity and air tightness of the material. In addition, compared with the traditional CVI process with its long cycle and high cost, the SiC prepared by RMI process f / SiC composite material process equipment is simple, production cycle is short, production cost is low, and large-sized structural parts can be formed to near net size. The present invention adopts a single RMI process to achieve Ti 3 SiC 2 Interface phase and Ti 3 SiC 2 Preparation of modified SiC matrix, for traditional SiC f The process improvement of SiC / SiC composite materials is revolutionary. The interface phase prepared by RMI process and the prepared matrix have better thermal adaptability, making SiC f The overall mechanical, radiation resistance and thermal physical properties of SiC composite materials can be greatly improved. Therefore, the present invention is a high-performance SiC composite material for nuclear use. f The new process for preparing SiC / SiC composite materials has great potential for application in structural materials of future advanced nuclear energy systems.

[0022] The first aspect of the present invention provides a new type of high-performance SiC f A method for preparing a SiC / SiC composite material, using a single reaction melt infiltration process to sequentially prepare an interface phase and a matrix phase of the composite material, comprising the following steps: The two-dimensional SiC fibers were placed in a magnetron sputtering instrument using SiC targets and TiO 2The target material is co-sputtered to form a Ti-Si-CO interface layer on the surface of the SiC fiber to obtain a two-dimensional SiC f / Ti-Si-CO fiber cloth; the Ti-Si-CO interface layer prepared on the fiber surface in this step is the target Ti 3 SiC 2 The interface layer precursor reacts with Si to form Ti in the subsequent gas phase siliconization step. 3 SiC 2 .

[0023] Two-dimensional SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f / Ti-Si-CO fiber cloth was placed in a graphite crucible, and Si powder was placed at the bottom of the graphite crucible. The temperature was raised to 1450-1500 °C and kept for 30-60 min to obtain SiC f / Ti 3 SiC 2 Interface phase two-dimensional fiber cloth; this step is the RMI process gas phase siliconization to obtain SiC f / Ti 3 SiC 2 The Si powder placed at the bottom of the crucible evaporates after the heating temperature exceeds the melting point of 1410 ℃, and the Si vapor diffuses into the two-dimensional SiC fiber cloth through the holes on the graphite plate, reacts with the Ti-Si-CO precursor prepared on the fiber surface in the previous step, and generates Ti in situ. 3 SiC 2 Interface phase.

[0024] Add TiC, TiO 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 Mix the reaction aids and ball mill to obtain a slurry suspension; TiC, TiO 2 The mixed powder is SiC-Ti prepared by RMI process 3 SiC 2 The precursor of the matrix is ​​made into a slurry suspension to fully fill the pores in and between the fiber bundles.

[0025] SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth is immersed in the slurry suspension to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2Fiber cloth; SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The fiber cloth is stacked to form a layered preform, and the layered preform is axially pressed and dried to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Green body; the purpose of this step is to laminate and shape the two-dimensional fiber cloth to obtain a compact two-dimensional sheet.

[0026] SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The green body is treated at 1200 ~ 1400℃ for 2~4h in an inert atmosphere or under vacuum conditions to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Preform; the purpose of this step is to obtain a certain mechanical strength of the plate through heat treatment to ensure that no deformation and breakage occurs during the subsequent RMI siliconization process.

[0027] SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1250-1450℃ for 30-60 min in a vacuum furnace to obtain Ti 3 SiC 2 Modified SiC matrix phase to obtain dense SiC f / Ti 3 SiC 2 Interface / SiC-Ti 3 SiC 2 Composite material, namely a new type of nuclear high-performance SiCf / SiC composite material, this step adopts RMI process liquid phase siliconization to obtain a new type of nuclear high-performance SiC f / SiC composite materials.

[0028] The dextrin solution is prepared by adding dextrin at a mass fraction of 0.1 to 1.0 wt.% into distilled water.

[0029] The TiC, TiO 2 The mixed raw materials include TiC powder and TiO 2 Powder; TiC powder and TiO 2The powder molar ratio is 1:1 to 3:1; the TiC powder and TiO 2 The particle diameter of the powder is 5-8 μm; the TiC powder is replaced by a mixed powder of Ti powder and C powder.

[0030] The Y 2 O 3 、Al 2 O 3 Mixed reaction aids include Y 2 O 3 Powder and Al 2 O 3 Powder; Y 2 O 3 Powder and Al 2 O 3 The molar ratio of powder is 2:1~1:2; Y 2 O 3 Powder and Al 2 O 3 The particle diameter of the powder is 10-12 μm.

[0031] Add TiC, TiO 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aid is mixed, and the mass of the mixed powder is 30-50 wt.% of the mass of the solution.

[0032] SiC f / Ti 3 SiC 2 The interfacial phase two-dimensional fiber cloth is immersed in the slurry suspension for 5 to 30 minutes.

[0033] When axial pressure is applied to the layered preform, the axial pressure is 5 to 20 MPa and the pressure is maintained for 5 to 30 minutes.

[0034] The drying temperature is 110~125℃ and the drying time is 24~48h.

[0035] The AlSi alloy powder is replaced with Si powder, ZrSi alloy powder or YSi alloy powder.

[0036] In one embodiment, a high performance SiC core is provided. f / SiC composite material preparation method, see Figure 1 As shown, using two-dimensional SiC fiber cloth, SiC target with 99% purity and TiO 2 The target material is TiC powder and TiO with a particle diameter of 5-8 μm and a molar ratio of 3:1 to 1:1.2 Powder mixed powder as raw material, with particle diameter of 10-12 μm and molar ratio of 2:1 ~ 1:2 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 10:1 to 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target are co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 ~ 5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f / Ti-Si-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1450~1500℃ and kept for 30~60 minutes to prepare SiC f / Ti 3 SiC 2 Interfacial phase two-dimensional fiber cloth; Step 3: Add dextrin into distilled water at a mass fraction of 0.1 to 1.0 wt.%, and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 Mix the reaction aids, add the mixed powder to the solution in an amount of 30 to 50 wt.% of the solution mass, and then place the mixture in a ball mill for 24 to 48 hours to obtain a uniform slurry suspension; Step 5: SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth is immersed in the above slurry suspension, and taken out after standing for 5 to 30 minutes to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Fiber cloth; Step 6: 2D SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2The fiber cloth is stacked and fixed with a flat mold up and down. An axial pressure of 5 to 20 MPa is applied. After holding the pressure for 5 to 30 minutes, the press is taken out and placed in an oven at 120 °C for 48 hours to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Greenware; Step 7: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1200 ~ 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Prefabricated body; Step 8: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The preform is embedded in AlSi alloy powder and kept at 1200 ~ 1450 ℃ in a vacuum furnace for 30 ~ 60 minutes to obtain dense SiC f / Ti 3 SiC 2 Interface / SiC-Ti 3 SiC 2 Composite materials.

[0037] The TiC powder used as the raw material in step 4 can be replaced by a mixed powder of Ti powder and C powder; The AlSi alloy powder used in steps 2 and 8 can be replaced by Si powder or other types of Si-containing alloys, such as ZrSi, YSi alloy, etc. The AlSi alloy powder in the present invention is used only to provide Si element, so alloys containing Si element are theoretically possible to be used; The vacuum furnace used in step 8 to perform the RMI process to infiltrate AlSi alloy powder can be replaced by a "tube furnace or box furnace used in a gas-tight, inert atmosphere."

[0038] It can be seen that the present invention uses a single RMI process to prepare Ti 3 SiC 2 Interface phase and Ti 3 SiC 2 Modified SiC matrix, the present invention innovatively selects TiO 2The target and SiC target were co-sputtered on the surface of SiC fiber to prepare the interface layer prefabricated phase, and the silicon was infiltrated by combining the gas phase RMI process to prepare Ti in situ reaction. 3 SiC 2 In the RMI preform shaping stage, the present invention selects to use the prepreg process to directly impregnate TiC, TiO 2 The two-dimensional SiC fiber cloth of the mixed slurry is laminated and pressed to shape, and then heat treated to give the preform a certain structural strength to ensure the structural integrity of the composite material in the subsequent RMI process.

[0039] The second aspect of the present invention provides a new type of high-performance SiC f / SiC composite materials.

[0040] A third aspect of the present invention provides a high performance SiC f / Application of SiC composite materials in nuclear industry.

[0041] It should be noted that the experimental methods used in the present invention are all conventional methods unless otherwise specified; the reagents and materials used are all commercially available unless otherwise specified.

[0042] Example 1 A high-performance SiC for nuclear applications f A new process for preparing / SiC composite materials, the preparation flow chart is as follows Figure 1 As shown, using two-dimensional SiC fiber cloth, SiC target with 99% purity and TiO 2 The target material is TiC powder with a particle diameter of 5 μm and a molar ratio of 2:1 and TiO 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target were co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f The Ti-Si-CO / Ti-Si-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1450 °C and kept for 30 minutes to prepare SiC f / Ti3 SiC 2 Interfacial phase two-dimensional fiber cloth; Step 3: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 5: SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth was immersed in the above slurry suspension and taken out after standing for 20 minutes to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Fiber cloth; Step 6: 2D SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The fiber cloth was stacked and fixed with a flat mold. An axial pressure of 10 MPa was applied. After holding the pressure for 5 minutes, the press was taken out and placed in an oven at 120 °C for 48 hours to obtain SiC. f / Ti 3 SiC 2 Interface / TiC-TiO 2 Greenware; Step 7: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Prefabricated body; Step 8: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1250 °C in a vacuum furnace for 30 minutes to obtain a dense SiC f / Ti 3 SiC 2 Interface / SiC-Ti 3 SiC 2 Composite materials, such as Figure 2 shown.

[0043] Figure 2 The dense SiC prepared in Example 1 f / Ti 3 SiC 2 Interface / SiC-Ti 3 SiC 2 Composite material physical picture; Figure 2 (a) and (b) are pictures taken from different directions. As shown in the figure, the sample has a compact structure, a metallic luster on the surface, and the two-dimensional SiC fiber cloth laminate can be clearly seen in the cross section.

[0044] Figure 3 The new high-performance nuclear SiC prepared in Example 1 f / SiC composite material microstructure image. Among them, Figure 3 (a) and (b) Microscopic images of the composite material at different magnifications. Figure 3 It can be seen that the new high-performance nuclear SiC f / SiC composite material is composed of SiC fiber, Ti 3 SiC 2 Interface phase and Ti 3 SiC 2 Modified SiC matrix composition; Ti introduced by RMI process can be seen at low magnification 3 SiC 2 The modified SiC matrix achieves complete filling of large-sized pores in the matrix, which intuitively illustrates that the RMI process adopted by the present invention achieves a complete filling of large-sized pores in the matrix. f / SiC composite material density improvement.

[0045] Example 2 A high-performance SiC for nuclear applications f A new process for preparing / SiC composite materials, the preparation flow chart is as follows Figure 1 As shown, using two-dimensional SiC fiber cloth, SiC target with 99% purity and TiO 2 The target material is TiC powder with a particle diameter of 5 μm and a molar ratio of 2:1 and TiO 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target were co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f The Ti-Si-CO / Ti-Si-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1450 °C and kept for 30 minutes to prepare SiC f / Ti 3 SiC 2 Interfacial phase two-dimensional fiber cloth; Step 3: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 5: SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth was immersed in the above slurry suspension and taken out after standing for 20 minutes to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Fiber cloth; Step 6: 2D SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The fiber cloth was stacked and fixed with a flat mold. An axial pressure of 10 MPa was applied. After holding the pressure for 5 minutes, the press was taken out and placed in an oven at 120 °C for 48 hours to obtain SiC. f / Ti 3 SiC 2 Interface / TiC-TiO 2 Greenware; Step 7: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Prefabricated body; Step 8: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1350 °C in a vacuum furnace for 30 minutes to obtain a dense SiC f / Ti 3 SiC 2 Interface / SiC-Ti 3 SiC 2 Composite materials.

[0046] Example 3 A high-performance SiC for nuclear applications f A new process for preparing / SiC composite materials, the preparation flow chart is as follows Figure 1 As shown, using two-dimensional SiC fiber cloth, SiC target with 99% purity and TiO 2 The target material is TiC powder with a particle diameter of 5 μm and a molar ratio of 2:1 and TiO 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target were co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f The Ti-Si-CO / Ti-Si-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1450 °C and kept for 30 minutes to prepare SiC f / Ti 3 SiC 2Interfacial phase two-dimensional fiber cloth; Step 3: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 5: SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth was immersed in the above slurry suspension and taken out after standing for 20 minutes to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Fiber cloth; Step 6: 2D SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The fiber cloth was stacked and fixed with a flat mold. An axial pressure of 10 MPa was applied. After holding the pressure for 5 minutes, the press was taken out and placed in an oven at 120 °C for 48 hours to obtain SiC. f / Ti 3 SiC 2 Interface / TiC-TiO 2 Greenware; Step 7: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Prefabricated body; Step 8: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1450℃ in a vacuum furnace for 30 minutes to obtain dense SiC f / Ti 3 SiC2 Interface / SiC-Ti 3 SiC 2 Composite materials.

[0047] Example 4 A high-performance SiC for nuclear applications f A new process for preparing / SiC composite materials, the preparation flow chart is as follows Figure 1 As shown, using two-dimensional SiC fiber cloth, SiC target with 99% purity and TiO 2 The target material is TiC powder with a particle diameter of 5 μm and a molar ratio of 2:1 and TiO 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target were co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f The Ti-Si-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1500 °C and kept for 30 minutes to prepare SiC f / Ti 3 SiC 2 Interfacial phase two-dimensional fiber cloth; Step 3: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 5: SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth was immersed in the above slurry suspension and taken out after standing for 20 minutes to obtain SiCf / Ti 3 SiC 2 Interface / TiC-TiO 2 Fiber cloth; Step 6: 2D SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The fiber cloth was stacked and fixed with a flat mold. An axial pressure of 10 MPa was applied. After holding the pressure for 5 minutes, the press was taken out and placed in an oven at 120 °C for 48 hours to obtain SiC. f / Ti 3 SiC 2 Interface / TiC-TiO 2 Greenware; Step 7: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 Prefabricated body; Step 8: SiC f / Ti 3 SiC 2 Interface / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1250 °C in a vacuum furnace for 30 minutes to obtain a dense SiC f / Ti 3 SiC 2 Interface / SiC-Ti 3 SiC 2 Composite materials.

[0048] Comparative Example 1 Two-dimensional SiC fiber cloth was used to prepare TiC powder and TiO with a particle diameter of 5 μm and a molar ratio of 2:1. 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth on a porous graphite plate and send it into a CVI chemical deposition furnace to prepare a PyC interface layer. Deposit at 900 °C for 72 h to obtain a PyC interface layer with a thickness of 0.5 μm on the surface of the SiC fiber. Step 2: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 3: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 4: SiC f The two-dimensional fiber cloth with SiC / PyC interface phase was immersed in the above slurry suspension and taken out after standing for 20 minutes to obtain f / PyC interface / TiC-TiO 2 Fiber cloth; Step 5: 2D SiC f / PyC interface / TiC-TiO 2 The fiber cloth was stacked and fixed with a flat mold. An axial pressure of 10 MPa was applied. After holding the pressure for 5 minutes, the press was taken out and placed in an oven at 120 °C for 48 hours to obtain SiC. f / PyC interface / TiC-TiO 2 Greenware; Step 6: SiC f / PyC interface / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / PyC interface / TiC-TiO 2 Prefabricated body; Step 7: SiC f / PyC interface / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1250℃ in a vacuum furnace for 30 minutes to obtain dense SiC f / PyC interface / SiC-Ti 3 SiC 2 Composite materials.

[0049] Comparative Example 2 Two-dimensional SiC fiber cloth was used to prepare TiC powder and TiO with a particle diameter of 5 μm and a molar ratio of 2:1. 2Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth on a porous graphite plate and send it into a CVI chemical vapor deposition furnace to prepare a PyC interface layer. Deposit at 900 °C for 72 h to obtain a PyC interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: SiC f The two-dimensional fiber cloth of the / PyC interface phase was stacked and fixed with a porous graphite flat mold and sent into a CVI chemical vapor deposition furnace to deposit the SiC matrix. The semi-dense porous SiC was obtained by deposition at 1000 °C for 360 h. f / PyC interface phase / SiC composite materials; Step 3: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 5: Porous SiC f The sample of the SiC / PyC interface phase / SiC composite material was immersed in the above slurry suspension and taken out after standing for 20 minutes to obtain the SiC f / PyC interface / SiC-TiC-TiO 2 Composite material preform; Step 6: SiC f / PyC interface / SiC-TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1250 °C in a vacuum furnace for 30 minutes to obtain a dense SiC f / PyC interface / SiC-Ti 3 SiC 2 Composite materials.

[0050] Comparative Example 3 Use two-dimensional SiC fiber cloth and prepare it according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth on a porous graphite plate and send it into a CVI chemical vapor deposition furnace to prepare a PyC interface layer. Deposit at 900 °C for 72 h to obtain a PyC interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: SiC f The two-dimensional fiber cloth of the PyC interface phase was stacked and fixed with a porous graphite flat mold, and then sent into a CVI chemical vapor deposition furnace to deposit the SiC matrix. The SiC matrix was deposited at 1000 °C for 1200 h to obtain a dense SiC f / PyC interface phase / SiC composite materials.

[0051] Comparative Example 4 Using two-dimensional SiC fiber cloth, 99% pure SiC target and TiO 2 The target material is TiC powder with a particle diameter of 5 μm and a molar ratio of 2:1 and TiO 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target were co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f The Ti-Si-CO / Ti-Si-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1450 °C and kept for 30 minutes to prepare SiC f / Ti 3 SiC 2 Interfacial phase two-dimensional fiber cloth; Step 3: SiC f / Ti 3 SiC 2 The interface phase two-dimensional fiber cloth is stacked, fixed with a porous graphite flat mold, and sent into a CVI chemical vapor deposition furnace to deposit the SiC matrix. The SiC matrix is ​​deposited at 1000 °C for 1200 h to obtain a dense SiC f / Ti 3 SiC 2 Interface phase / SiC composite material.

[0052] Comparative Example 5 Using two-dimensional SiC fiber cloth, 99% pure SiC target and TiO 2 The target material is TiC powder with a particle diameter of 5 μm and a molar ratio of 2:1 and TiO 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target were co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f The Ti-Si-CO / Ti-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1400 °C and kept for 30 minutes to prepare a TiO 2 +Two-dimensional SiC fiber cloth with TiC interface phase; Step 3: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2 Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 5: Immerse the two-dimensional SiC fiber cloth with the interface phase in the above slurry suspension, let it stand for 20 minutes and then take it out to obtain a two-dimensional SiC fiber cloth with TiC-TiO 2 Two-dimensional SiC fiber cloth; Step 6: Attach TiC-TiO 2 The two-dimensional SiC fiber cloth was stacked, fixed with a flat mold up and down, and an axial pressure of 10 MPa was applied. After holding the pressure for 5 minutes, it was taken out from the press and placed in an oven at 120 °C for 48 hours to obtain SiC f / TiO 2 +TiC interface phase / TiC-TiO 2 Greenware; Step 7: SiC f / TiO 2 +TiC interface phase / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / TiO 2 +TiC interface phase / TiC-TiO 2 Prefabricated body; Step 8: SiC f / TiO 2 +TiC interface phase / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1250 °C in a vacuum furnace for 30 minutes to obtain a dense SiC f / TiO 2 +TiC interface phase / SiC-Ti 3 SiC 2 Composite materials.

[0053] Comparative Example 6 Using two-dimensional SiC fiber cloth, 99% pure SiC target and TiO 2 The target material is TiC powder with a particle diameter of 5 μm and a molar ratio of 2:1 and TiO 2 Powder mixed powder was used as raw material, with a particle diameter of 10 μm and a molar ratio of 1:1. 2 O 3 and Al 2 O 3 The mixed powder is a reaction aid, the mass ratio of the raw material mixed powder to the reaction aid mixed powder is 20:1, and is prepared according to the following steps: Step 1: Place the two-dimensional SiC fiber cloth in a magnetron sputtering instrument and use TiO 2 The target and SiC target were co-sputtered to prepare a Ti-Si-CO interface layer with a thickness of 0.5 μm on the surface of the SiC fiber; Step 2: 2D SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f The Ti-Si-CO / Ti-Si-CO fiber cloth was placed in a graphite crucible, Si powder was placed at the bottom of the graphite crucible, and the temperature was raised to 1550 °C and kept for 30 minutes to prepare a TiSi 2 +Two-dimensional SiC fiber cloth with SiC interface phase; Step 3: Add dextrin at a mass fraction of 0.5 wt.% into distilled water and stir thoroughly to obtain a solution; Step 4: Add TiC and TiO to the above solution in sequence. 2Mix raw materials and Y 2 O 3 、Al 2 O 3 The reaction aids were mixed, and the mass of the mixed powder added to the solution was 30 wt.% of the mass of the solution, and then the mixture was placed in a ball mill for 24 hours to obtain a uniform slurry suspension; Step 5: Immerse the two-dimensional SiC fiber cloth with the interface phase in the above slurry suspension, let it stand for 20 minutes and then take it out to obtain a two-dimensional SiC fiber cloth with TiC-TiO 2 Two-dimensional SiC fiber cloth; Step 6: Attach TiC-TiO 2 The two-dimensional SiC fiber cloth was stacked, fixed with a flat mold up and down, and an axial pressure of 10 MPa was applied. After holding the pressure for 5 minutes, it was taken out from the press and placed in an oven at 120 °C for 48 hours to obtain SiC f / TiSi 2 +SiC interface phase / TiC-TiO 2 Greenware; Step 7: SiC f / TiSi 2 +SiC interface phase / TiC-TiO 2 The green body is placed in a vacuum furnace and heat treated at 1400 °C for 2 hours under inert atmosphere or vacuum conditions to obtain SiC f / TiSi 2 +SiC interface phase / TiC-TiO 2 Prefabricated body; Step 8: SiC f / TiSi 2 +SiC interface phase / TiC-TiO 2 The preform was embedded in AlSi alloy powder and kept at 1250 °C in a vacuum furnace for 30 minutes to obtain a dense SiC f / TiSi 2 +SiC interface phase / SiC-Ti 3 SiC 2 Composite materials.

[0054] In order to illustrate the new high performance SiC f The relevant properties of the preparation method of the SiC composite material are explained in combination with the embodiments and comparative examples.

[0055] It should be noted that the differences in microstructural features such as grain arrangement and porosity between phases prepared by different preparation processes result in differences in thermal expansion coefficients even for the same material. This difference causes internal stress to maintain the phase balance of the object between phases prepared by different processes after the material is lowered from the preparation temperature to room temperature, i.e., residual thermal stress. For ceramic-based composites, a large number of microcracks will be generated in the matrix under the action of residual thermal stress, which greatly reduces the strength and fracture toughness of the material.

[0056] SiC was prepared by RMI process f Ti in SiC composites 3 SiC 2 Interface phase and Ti 3 SiC 2 The matrix can greatly reduce the residual stress caused by preparing the interface phase and the matrix separately by different preparation processes, such as using a combination of different processes such as "CVI process to prepare the interface phase + RMI process to prepare the matrix phase", "RMI process to prepare the interface phase + CVI process to prepare the matrix phase", or "molten salt process to prepare the interface phase + CVI process to prepare the matrix phase", as shown in Table 1.

[0057] Table 1 shows SiC prepared by different processes f Comparison of performance parameters of SiC composite materials

[0058] As can be seen from Table 1, compared with traditional nuclear SiC f / SiC composite material, the new composite material proposed by the invention has high density and low porosity, and the SiC prepared by CVI process f The open porosity of the / SiC composite material was reduced from 10-13% to less than 3%, further improving the flexural strength of the material; compared with the SiC prepared by the CVI combined with RMI hybrid preparation process f / SiC composite material, the new composite material prepared by the single RMI process proposed in the present invention has higher bending strength, up to 700 MPa or more, and fracture toughness up to 25 MPa·m 1 / 2 Compared with the PyC interface, TiO 2 +TiC interface and TiSi 2 +SiC interface SiC f / SiC composite material, the present invention proposes to use Ti 3 SiC 2 The new composite material with interface has better fracture toughness.

[0059] The present invention adopts RMI process to prepare Ti 3 SiC 2Interface phase and Ti 3 SiC 2 Compared with combined process modification methods such as CVI+RMI or CVI+PIP+RMI, the unified interface phase and matrix preparation method can greatly improve the thermal adaptation between the interface phase and the matrix, reduce the residual stress in the composite material, and improve the mechanical strength of the material; the present invention adopts the RMI process to replace the traditional CVI process preparation method, and the process cycle is shortened to one tenth of the traditional CVI process cycle, and the production cost is greatly reduced; the product prepared by the RMI process can achieve near-net size molding, which is suitable for the preparation of large-sized special-shaped composite material components.

[0060] The present invention proposes to use Ti 3 SiC 2 Interface phase replaces traditional core SiC f The PyC interface phase in the Ti / SiC composite material can effectively prevent the amorphization failure of the traditional interface phase during irradiation service, which ultimately leads to a significant attenuation of the mechanical properties of the composite material. 3 SiC 2 The introduction of the interface phase greatly improves the SiC f / SiC composite materials’ radiation resistance and mechanical strength retention during service; The present invention proposes that SiC f Use of Ti in SiC composite matrix 3 SiC 2 Replace part of the SiC matrix, in Ti 3 SiC 2 Under the effect of modified matrix, SiC f The overall fracture toughness of the SiC composite material is further improved.

[0061] The present invention describes preferred embodiments and their effects. However, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0062] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A new type of high-performance SiC for nuclear applications f A method for preparing a SiC composite material, characterized in that: The composite material interface phase and matrix phase are prepared in sequence using a single reaction melt infiltration process, including the following steps: The two-dimensional SiC fiber was placed in a magnetron sputtering instrument, and a SiC target and a TiO2 target were used for co-sputtering to obtain a Ti-Si-CO interface layer on the surface of the SiC fiber. f / Ti-Si-CO fiber cloth; Two-dimensional SiC f / Ti-Si-CO fiber cloth was transferred to a porous graphite plate, and then the two-dimensional SiC f / Ti-Si-CO fiber cloth was placed in a graphite crucible, and Si powder was placed at the bottom of the graphite crucible. The temperature was raised to 1450-1500 °C and kept for 30-60 min to obtain SiC f / Ti3SiC2 interface phase two-dimensional fiber cloth; Add TiC and TiO2 mixed raw materials and Y2O3 and Al2O3 mixed reaction aids to the dextrin solution in sequence, and obtain a slurry suspension by ball milling. SiC f / Ti3SiC2 interface phase two-dimensional fiber cloth is immersed in the slurry suspension to obtain SiC f / Ti3SiC2 interface / TiC-TiO2 fiber cloth; SiC f / Ti3SiC2 interface / TiC-TiO2 fiber cloth is stacked to form a layered preform, and the layered preform is axially pressed and dried to obtain SiC f / Ti3SiC2 interface / TiC-TiO2 green body; SiC f / Ti3SiC2 interface / TiC-TiO2 green body, in an inert atmosphere or under vacuum conditions, at 1200 ~ 1400 ℃ for 2 ~ 4h to obtain SiC f / Ti3SiC2 interface / TiC-TiO2 preform; SiC f / Ti3SiC2 interface / TiC-TiO2 preform is embedded in AlSi alloy powder and kept at 1250~1450℃ in a vacuum furnace for 30~60min to obtain SiC matrix phase modified by Ti3SiC2, that is, a new type of high-performance SiC for nuclear use is obtained. f / SiC composite materials.

2. The novel high-performance SiC for nuclear use according to claim 1 f A method for preparing a SiC composite material, characterized in that: The dextrin solution is prepared by adding dextrin in a mass fraction of 0.1 to 1.0 wt.% into distilled water.

3. The novel high-performance SiC for nuclear use according to claim 1 f A method for preparing a SiC composite material, characterized in that: The TiC and TiO2 mixed raw material comprises TiC powder and TiO2 powder; Wherein, the molar ratio of TiC powder to TiO2 powder is 1:1~3:1; The particle diameters of the TiC powder and the TiO2 powder are both 5-8 μm.

4. The novel high-performance SiC for nuclear use according to claim 3 f A method for preparing a SiC composite material, characterized in that: The TiC powder is replaced with a mixed powder of Ti powder and C powder.

5. The novel high-performance SiC for nuclear use according to claim 1 f A method for preparing a SiC composite material, characterized in that: The Y2O3 and Al2O3 mixed reaction aid comprises Y2O3 powder and Al2O3 powder; Wherein, the molar ratio of Y2O3 powder to Al2O3 powder is 2:1~1:2; The particle diameters of Y2O3 powder and Al2O3 powder are both 10-12 μm.

6. The novel high-performance SiC for nuclear use according to claim 1 f A method for preparing a SiC composite material, characterized in that: TiC and TiO2 mixed raw materials and Y2O3 and Al2O3 mixed reaction aids are added to the dextrin solution in sequence, and the mass of the mixed powder is 30-50 wt.% of the mass of the solution.

7. The novel high-performance SiC for nuclear use according to claim 1 f A method for preparing a SiC composite material, characterized in that: SiC f / Ti3SiC2 interface phase two-dimensional fiber cloth is immersed in the slurry suspension for 5 to 30 min; When axial pressure is applied to the layered preform, the axial pressure is 5 to 20 MPa and the pressure is maintained for 5 to 30 minutes; the temperature during drying is 110 to 125°C and the drying time is 24 to 48 hours.

8. The novel high-performance SiC for nuclear use according to claim 1 f A method for preparing a SiC composite material, characterized in that: The AlSi alloy powder is replaced with Si powder, ZrSi alloy powder or YSi alloy powder.

9. A novel high-performance SiC for nuclear use obtained by the method according to any one of claims 1 to 8 f / SiC composite materials.

10. A high performance SiC as claimed in claim 9 f / Application of SiC composite materials in nuclear industry.

Citation Information

Patent Citations

  • Preparation method of Ti3SiC2 interface layer-containing SiCf / Si composite

    CN109467450A

  • Method for preparing SiCf / Si-Y-B-C composite material by combining vacuum impregnation with reactive melt impregnation

    CN114656275A

  • Silicon carbide reinforced silicon carbide composite material and preparation method thereof

    CN117800750A

Cited By

  • High-temperature-resistant nuclear fuel cladding tube based on porous interface and intelligent manufacturing method of high-temperature-resistant nuclear fuel cladding tube