Lead azide / conducting polymer as well as preparation method and application thereof

The lead azide/conductive polymer is prepared through acoustic resonance mixing technology, which solves the problems of uneven mixing and safety hazards in the traditional stirring paddle mixing method, achieves efficient and uniform preparation of lead azide/conductive polymer, and reduces the cost of Static sensitivity improves product quality and reaction safety.

CN118754792APending Publication Date: 2024-10-11CHINA WANBAO ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410817409.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The traditional stirring paddle mixing method to prepare lead azide and ignition powder lead styphnate complex has the problems of uneven mixing, low efficiency, uneven products and safety hazards, and it is difficult to effectively reduce the electrostatic sensitivity of lead azide.

Method used

Lead azide/conductive polymer is prepared using acoustic resonance mixing technology. By setting up an acoustic resonance platform and reaction vessel, the resonance frequency and phase difference are adjusted to achieve a full range of material mixing, reduce the shear force and friction of the reaction materials, and improve Reaction safety and product homogeneity.

Benefits of technology

The reaction efficiency and product uniformity are significantly improved, the electrostatic sensitivity of lead azide is reduced, the product quality and yield are improved, the electrostatic sensitivity can be reduced to 1.3J, and the reaction safety is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754792A_ABST
    Figure CN118754792A_ABST
Patent Text Reader

Abstract

The invention discloses a lead azide / conductive polymer and a preparation method and application thereof. The preparation method comprises the following steps: preparing a lead nitrate solution with a first set concentration, dropwise adding dilute nitric acid, adjusting the pH value to a set value, and preparing a sodium azide solution; after the reaction container is installed on an acoustic resonance platform, the resonance frequency and the phase difference of the resonance frequency are adjusted, the acceleration of the acoustic resonance reaction platform is kept within a set range, after the lead nitrate solution and the sodium azide solution are added into the reaction container for a reaction, the reaction container is heated, and then the reaction is conducted for a set duration; and after the reaction is finished, filtering the obtained turbid liquid to obtain a filtered substance, washing the filtered substance, and drying to obtain the lead azide. The lead azide and the pyrrole dispersion liquid are placed on a second acoustic resonance reaction platform for reaction, the lead azide / conductive polymer is obtained, the sensitivity is lower, the polymer is safer, and the preparation efficiency is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to an energetic material and a preparation technology thereof, and in particular to a lead azide / conductive polymer and a preparation method and use thereof. Background Art

[0002] The explosive is the core charge of pyrotechnics such as detonators. It can quickly realize the transition from combustion to detonation and then detonate the next level of charge. It is widely used in civilian blasting devices, aerospace systems, military weapon systems and space pyrotechnics. Lead azide (LA) is an excellent explosive with good stability, fast detonation growth, high detonation ability, not easy to decompose, and non-hygroscopicity, and has a very high application prospect. However, it has high electrostatic sensitivity and poor ignition ability. It needs to be used with ignition powder lead styphnate (LS) to achieve ignition and detonation by using the high electrostatic sensitivity of LS. At present, the modification methods of LA and LS are mainly: adding crystal shape controllers to control their crystal shape or adding conductive carbon materials such as graphene to adjust their sensitivity. These modification methods effectively improve their sensitivity performance. However, the method of preparing LA composites and LS composites by mixing with traditional stirring impellers has the disadvantages of uneven mixing, large amount of work-in-progress, low efficiency, uneven products, and safety hazards in the preparation process. Summary of the invention

[0003] In view of this, the embodiments of the present application provide a lead azide / conductive polymer and a preparation method and use thereof, so as to at least solve the above-mentioned technical problems.

[0004] According to the first aspect of the present application, a method for preparing lead azide / conductive polymer is provided, comprising: Preparing a lead nitrate solution of a first set concentration, dropping dilute nitric acid into it, and adjusting the pH value of the lead nitrate solution to a set value; preparing a sodium azide solution with a second set concentration; After installing the first reaction container on the first acoustic resonance platform, adjusting the resonance frequency and phase difference of the first acoustic resonance reaction platform so that the acceleration of the first acoustic resonance reaction platform is maintained within a first set range, and adding the lead nitrate solution and the sodium azide solution into the reaction container respectively; After reacting for a first set time, heating the first reaction container to a first set temperature, and then reacting for a second set time; After the reaction is completed, a suspension is obtained, the suspension is filtered to obtain a filtrate, the filtrate is washed with ethanol for multiple times, and then dried to obtain lead azide; Adding the prepared lead azide into an appropriate amount of distilled water, stirring and dispersing the lead azide evenly to obtain a lead azide dispersion, so that the lead azide in the lead azide dispersion reaches a third set concentration; adding pyrrole to an appropriate amount of ethanol to obtain a pyrrole dispersion, so that the pyrrole in the pyrrole dispersion reaches a fourth set concentration; After installing the second reaction container on the second acoustic resonance platform, adjusting the resonance frequency and phase difference of the second acoustic resonance reaction platform so that the acceleration of the second acoustic resonance reaction platform is maintained within a second set range, and respectively adding the lead azide dispersion and the pyrrole dispersion into the second reaction container; heating the second reaction container to a second set temperature; wherein the volume ratio of the lead azide dispersion to the pyrrole dispersion is 24:7 to 21:5; adding sodium dodecylbenzenesulfonate into the second reaction container, slowly adding a fifth set concentration FeCl3 solution placed in an ice bath into the second reaction container, allowing the mixed solution in the second reaction container to react at a third set temperature for a third set time, filtering, washing, and drying the reactants to obtain a core-shell structure composite material, namely, a lead azide / PPy composite material; The mass ratio of the sodium dodecylbenzene sulfonate to the lead azide dispersion is 1:100 to 1:105, and the mass ratio of the FeCl3 solution to the lead azide dispersion is 1:24 to 1:26.

[0005] In some optional embodiments, the first set concentration is: 0.02g / mL~3g / mL; the second set concentration is: 0.05g / mL~6g / mL; the third set concentration is: 0.9g / mL~2.3g / mL; the fourth set concentration is: 0.06g / mL~0.11g / mL; the fifth set concentration is: 0.0032mol / mL~0.0048mol / mL.

[0006] In some optional embodiments, the set value is 2.6~3.2.

[0007] In some optional embodiments, the resonance frequency of the first acoustic resonance platform is 52-70 Hz; the phase difference of the first acoustic resonance platform ranges from 0.01 to 0.4; and the acceleration is maintained at 12 g to 185 g.

[0008] In some optional embodiments, the resonance frequency of the second acoustic resonance platform is 50-70 Hz; the phase difference of the second acoustic resonance platform ranges from 0.02 to 0.35; and the acceleration is maintained at 20 g to 175 g.

[0009] In some optional embodiments, the first set temperature is 25°C to 95°C; the second set temperature is 0°C to 2.5°C; and the third set temperature is 0°C to 1°C.

[0010] In some optional embodiments, the first set time length is 0.1 min to 2 min; the second set time length is 1 min to 120 min; and the third set time length is 1 min to 60 min.

[0011] In some optional embodiments, the content of PPy in the lead azide / PPy composite is 0.01wt%~16wt%, and the content of lead azide is 84wt%~99.99wt%.

[0012] According to a second aspect of the present application, a lead azide / conductive polymer is provided, wherein the lead azide / conductive polymer is prepared by the above-mentioned lead azide / conductive polymer preparation method.

[0013] According to a third aspect of the present application, a use of lead azide / conductive polymer is provided, wherein the lead azide / conductive polymer is used as an explosive.

[0014] Compared with the traditional preparation method of the stirring paddle, the mixed preparation technology of the embodiment of the present application reduces the shear force of the reaction materials in the mixing, avoids the friction between the materials, stirring paddles and reaction vessels, improves the intrinsic safety of the reaction, and greatly shortens the reaction time, effectively reduces energy consumption, and has a higher product yield, and better product uniformity and quality. By adjusting the different contents of the conductive polymer and lead azide compound, the electrostatic sensitivity and mechanical sensitivity of lead azide are effectively reduced. The PPy of the embodiment of the present application has high conductivity. By the method of acoustic resonance mixing, a LA / PPy core-shell complex uniformly coated on the surface of LA can be obtained. Due to the coating effect of PPy, the sensitivity of LA can be effectively regulated. The embodiment of the present application reduces the shear force of the reaction materials in the mixing, avoids the friction between the materials, stirring paddles and reaction vessels, and improves the intrinsic safety of the reaction; by setting the acoustic resonance platform and the reaction vessel, the reaction time is greatly shortened, the energy consumption is effectively reduced, the product yield is higher, and the product uniformity and quality are better. By adjusting the different contents of conductive polymer and lead azide composite, the electrostatic sensitivity of lead azide can be effectively reduced to 1.3J. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A schematic flow chart of the method for preparing lead azide / conductive polymer provided in an embodiment of the present application. DETAILED DESCRIPTION

[0016] The essence of the technical solution of the embodiment of the present application is explained in detail below.

[0017] The embodiment of the present application adopts the acoustic resonance mixing preparation technology to prepare lead azide / conductive polymer, mainly using the exciter to produce mechanical vibration to form mechanical waves; further using the spring system to transmit the mechanical waves to the reactor, the materials in the reactor can produce macroscopic vibration mixing and micro-mixing of sound waves. The micro-mixing effect of sound waves can be distributed throughout the reactor, which is dead-angle-free and omnidirectional, and belongs to full-field mixing. Compared with the traditional preparation method of stirring paddles, this mixing preparation technology has more complete mixing between the reaction materials, faster reaction speed, and better and more uniform quality of the reaction product. PPy has high conductivity. Through the method of acoustic resonance mixing, a lead azide / PPy (polypyrrole) core-shell complex uniformly coated on the surface of lead azide can be obtained. Due to the coating effect of PPy, the electrostatic sensitivity and mechanical sensitivity of lead azide can be effectively regulated.

[0018] Figure 1 A schematic diagram of the preparation method of lead azide / conductive polymer provided in the embodiment of the present application, such as Figure 1 As shown, the preparation method of lead azide / conductive polymer provided in the embodiment of the present application comprises the following steps: Step 101, preparing a lead nitrate solution of a first set concentration, dropping dilute nitric acid into it, and adjusting the pH value of the lead nitrate solution to a set value.

[0019] In the embodiment of the present application, the first set concentration can be 0.02 g / mL to 3 g / mL. As an example, the concentration of the lead nitrate solution can be 0.03 g / mL, 0.06 g / mL, 0.09 g / mL, 0.10 g / mL, 0.13 g / mL, 0.16 g / mL, 0.18 g / mL, 0.20 g / mL, 0.24 g / mL, 0.32 g / mL, 0.40 g / mL, 0.60 g / mL, 0.75 g / mL, 1 g / mL, 1.20 g / mL, 1.30 g / mL, 1.50 g / mL, 1.75 g / mL, 2 g / mL, 2.25 g / mL, 2.30 g / mL, 2.40 g / mL, 2.75 g / mL, 2.80 g / mL, 2.90 g / mL or 2.95 g / mL, etc.

[0020] In the embodiment of the present application, the dilute nitric acid may be nitric acid with a concentration of 0.95 wt % to 1.12 wt %.

[0021] In the embodiment of the present application, after the lead nitrate solution is prepared, its pH value needs to be adjusted so that the pH value of the lead nitrate solution is in the range of 2.6 to 3.2. Preferably, the pH value of the lead nitrate solution is 2.7, 2.8, 2.9, 3, or 3.1.

[0022] Step 102, preparing a sodium azide solution with a second set concentration.

[0023] In the embodiment of the present application, the second set concentration can be: 0.05g / mL to 6g / mL. As an example, the concentration of the sodium azide solution can be 0.07g / mL, 0.1g / mL, 0.14g / mL, 0.18g / mL, 0.25g / mL, 0.35g / mL, 0.60g / mL, 0.75g / mL, 0.85g / mL, 1g / mL, 1.20g / mL, 1.30g / mL, 1.50g / mL, 1.80g / mL, 2g / mL, 2.20g / mL, 2.40g / mL, 2.50g / mL , 2.80g / mL, 2.95g / mL, 3g / mL, 3.20g / mL, 3.40g / mL, 3.50g / mL, 3.60g / mL, 3.80g / mL, 4g / mL, 4.20g / mL, 4. 30g / mL, 4.50g / mL, 4.70g / mL, 4.90g / mL, 5g / mL, 5.10g / mL, 5.30g / mL, 5.50g / mL, 5.70g / mL, or 5.90g / mL, etc.

[0024] Step 103, after installing the first reaction container on the first acoustic resonance platform, adjusting the resonance frequency and phase difference of the first acoustic resonance reaction platform to keep the acceleration of the first acoustic resonance reaction platform within a first set range, and adding the lead nitrate solution and the sodium azide solution into the reaction container respectively.

[0025] In the embodiment of the present application, the phase difference of the first acoustic resonance reaction platform ranges from 0.01 to 0.4. As an implementation, the phase difference of the first acoustic resonance reaction platform can be 0.03, 0.05, 0.08, 0.10, 0.15, 0.18, 0.20, 0.24, 0.28, 0.3, 0.32, 0.35, 0.37, or 0.39, etc. As a preferred embodiment, the phase difference of the first acoustic resonance reaction platform can be 0.1 to 0.25. The resonant frequency of the first acoustic resonance reaction platform is 52Hz to 70Hz. As an implementation, the resonant frequency of the first acoustic resonance reaction platform is set to 54Hz, 56Hz, 58Hz, 60Hz, 63Hz, 65Hz, 68Hz, or 69Hz, etc. As a preferred embodiment, the resonant frequency of the first acoustic resonance reaction platform is preferably 60Hz to 65Hz. The acceleration of the first acoustic resonance reaction platform is 12g to 185g. Specifically, the acceleration of the first acoustic resonance reaction platform can be 15g, 20g, 22g, 25g, 27g, 30g, 35g, 42g, 45g, 50g, 55g, 60g, 66g, 70g, 75g, 80g, 85g, 95g, 105g, 110g, 115g, 120g, 125g, 130g, 135g, 145g, 155g, 165g, 175g, 180g, or 184g, etc. As a preferred embodiment, the acceleration of the acoustic resonance reaction platform is set to 60g-80g.

[0026] Step 104, after reacting for the first set time, the reaction container is heated to the first set temperature, and then reacted for the second set time.

[0027] In the embodiment of the present application, the first set time length can be 0.1min to 2min, specifically, the first set time length can be 0.2min, 0.3min, 0.6min, 1min, 1.2min, 1.5min, 1.8min, or 1.9min, etc. As long as the lead nitrate solution and the sodium azide solution are fully reacted, the first set time length can be longer.

[0028] The first set temperature can be 25℃~95℃. As an example, the first set temperature can be 27℃, 30℃, 33℃, 35℃, 38℃, 40℃, 42℃, 45℃, 47℃, 50℃, 55℃, 58℃, 60℃, 65℃, 70℃, 82℃, 85℃, 90℃, or 94℃, etc.

[0029] In the embodiment of the present application, the second set time length can be 1min to 120min. Specifically, the second set time length is set to ensure sufficient reaction between the lead nitrate solution and the sodium azide solution. When the lead nitrate solution and the sodium azide solution are fully mixed, the second set time length can be set to 5min, 8min, 10min, 12min, 16min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min, 60min, 65min, 70min, 75min, 70min, 80min, 85min, 90min, 95min, 100min, 115min, or 118min, etc. The second set time length can be set longer to allow the lead nitrate solution and the sodium azide solution to react more fully.

[0030] Step 105, after the reaction is completed, a suspension is obtained, the suspension is filtered to obtain a filtrate, the filtrate is washed with ethanol for multiple times, and then dried to obtain lead azide.

[0031] In the embodiment of the present application, the number of washing times can be 6 times, 8 times, etc.

[0032] Step 106, adding the prepared lead azide into an appropriate amount of distilled water, stirring and dispersing the lead azide evenly to obtain a lead azide dispersion, so that the lead azide in the lead azide dispersion reaches a third set concentration.

[0033] In the embodiment of the present application, the third set concentration is: 0.9 g / mL to 2.3 g / mL. As an example, the concentration of lead azide in the lead azide dispersion can be 0.95 g / mL, 1.0 g / mL, 1.05 g / mL, 1.2 g / mL, 1.3 g / mL, 1.4 g / mL, 1.5 g / mL, 1.6 g / mL, 1.7 g / mL, 1.8 g / mL, 1.9 g / mL, 2.0 g / mL, 2.1 g / mL, or 2.2 g / mL, etc.

[0034] Step 107, adding pyrrole to an appropriate amount of ethanol to obtain a pyrrole dispersion liquid, so that the pyrrole in the pyrrole dispersion liquid reaches a fourth set concentration.

[0035] In the embodiment of the present application, the fourth set concentration is: 0.06 g / mL to 0.11 g / mL. As an example, the concentration of pyrrole in the pyrrole dispersion can be 0.07 g / mL, 0.08 g / mL, 0.09 g / mL, 0.1 g / mL, or 0.105 g / mL.

[0036] Step 108, after installing the second reaction container on the second acoustic resonance platform, adjusting the resonance frequency and phase difference of the second acoustic resonance reaction platform to keep the acceleration of the second acoustic resonance reaction platform within a second set range, adding the lead azide dispersion and the pyrrole dispersion into the second reaction container respectively; and heating the second reaction container to a second set temperature.

[0037] In the embodiments of the present application, the volume ratio of the lead azide dispersion to the pyrrole dispersion is 24:7 to 21:5.

[0038] In the embodiment of the present application, the phase difference of the second acoustic resonance reaction platform ranges from 0.02 to 0.35. As an implementation method, the phase difference of the first acoustic resonance reaction platform can be 0.03, 0.05, 0.07, 0.09, 0.10, 0.12, 0.16, 0.18, 0.20, 0.23, 0.25, 0.27, 0.30, 0.32, or 0.34, etc. As a preferred method, the phase difference of the second acoustic resonance reaction platform can be 0.15 to 0.25. The resonant frequency of the second acoustic resonance reaction platform is 50 Hz to 70 Hz. As an implementation, the resonance frequency of the first acoustic resonance reaction platform is set to 50.5Hz, 51.3Hz, 51.7Hz, 52.6Hz, 53.5Hz, 55.4Hz, 57.4Hz, 58.5Hz, 59.5Hz, 60.5Hz, 61.5Hz, 62Hz, 62.5Hz, 63.5Hz, 63.9Hz, 64.5Hz, 64.9Hz, 65.5Hz, 66.0Hz, 67.5Hz, 68.8Hz, or 69.6Hz, etc. As a preferred embodiment, the resonance frequency of the second acoustic resonance reaction platform is preferably 60Hz to 66Hz. The acceleration of the second acoustic resonance reaction platform is 12g to 185g. Specifically, the acceleration of the second acoustic resonance reaction platform can be 16g, 20g, 25g, 30g, 35g, 45g, 48g, 50g, 55g, 60g, 65g, 70g, 75g, 80g, 85g, 90g, 95g, 100g, 108g, 115g, 120g, 125g, 130g, 135g, 140g, 152g, 157g, 160g, 165g, 172g, 175g, 180g, or 184g, etc. As a preferred embodiment, the acceleration of the acoustic resonance reaction platform is set to 60g-90g.

[0039] The second set temperature may be 0° C. to 2.5° C. As an example, the second set temperature may be 0.1° C., 0.3° C., 0.5° C., 0.8° C., 1° C., 1.5° C., 2° C., or 2.4° C., etc.

[0040] In the embodiment of the present application, the second acoustic resonance reaction platform and the first acoustic resonance reaction platform can be the same, that is, an acoustic resonance reaction platform with the same operating parameters is selected for the preparation reaction. However, considering the different shapes of the reaction substances, it is recommended to use the relevant operating parameters of the acoustic resonance reaction platform in the embodiment of the present application to prepare lead azide / conductive polymer.

[0041] Step 109, adding sodium dodecylbenzene sulfonate to the second reaction container, slowly adding the fifth set concentration FeCl3 solution placed in an ice bath condition to the second reaction container, allowing the mixed solution in the second reaction container to react at a third set temperature for a third set time, filtering, washing, and drying the reactants to obtain a core-shell structure composite material, namely, a lead azide / PPy composite material.

[0042] In the embodiments of the present application, the mass ratio of sodium dodecylbenzene sulfonate to the lead azide dispersion is 1:100 to 1:105, and the mass ratio of FeCl3 solution to the lead azide dispersion is 1:24 to 1:26.

[0043] In the embodiment of the present application, the third set temperature may be 0° C. to 1° C. As an example, the third set temperature may be 0.1° C., 0.2° C., 0.4° C., 0.5° C., 0.6° C., 0.8° C., or 0.9° C., etc.

[0044] In the embodiment of the present application, the third set time length may be 1 min to 60 min. As an example, the third set time length may be 5 min, 10 min, 15 min, 18 min, 20 min, 24 min, 28 min, 30 min, 32 min, 36 min, 408 min, 45 min, 48 min, 50 min, 54 min, 57 min, or 59 min, etc.

[0045] In the embodiment of the present application, the fifth set concentration is: 0.0032mol / mL~0.0048mol / mL. As an example, the concentration of the FeCl3 solution is 0.0033mol / mL, 0.0035mol / mL, 0.0038mol / mL, 0.004mol / mL, 0.0042mol / mL, 0.0044mol / mL, or 0.0047mol / mL, etc.

[0046] In the embodiments of the present application, the content of PPy in the lead azide / PPy composite is 0.01 wt % to 16 wt %, and the content of lead azide is 84 wt % to 99.99 wt %.

[0047] The technical scheme of the embodiment of the present application is described below in conjunction with specific examples, but the conditions and results described in the implementation do not limit the scope of protection of the present application. The embodiment of the present application only illustrates the preparation of lead azide, lead nitrate solution, etc. with exemplary contents. For industrial use or other preparation amounts, the amount can be expanded in proportion accordingly. The preparation device used is also only an exemplary description. In industrial production, alternative container equipment can be used, or the corresponding container equipment can be enlarged in proportion. Example

[0048] In this embodiment, first weigh 1.32g of sodium azide (NaN3) and dissolve it in 40mL of deionized water to obtain a sodium azide solution; weigh 1.65g of lead nitrate (Pb(NO3)2) and dissolve it in 40mL of deionized water, drop dilute nitric acid (concentration of 1%) to adjust the pH of the lead nitrate solution to 3 to obtain a lead nitrate solution; after the reaction container is installed on the acoustic resonance platform, the reaction container is fixed, the resonance frequency is set to 63.8Hz, the phase difference is set to 0.02, the acceleration G1 is 60g, and the above-configured lead nitrate solution and sodium azide solution are respectively added to the reaction container by a metering pump, the materials in the reaction container are reacted at room temperature for 1min, the temperature of the reaction system is raised to 65°C, and the reaction is continued at 65°C for 10min; after the reaction is completed, cool and filter, and the obtained lead azide The mixture was washed with deionized water and ethanol in turn, and dried in a vacuum drying oven to obtain a dry lead azide product; 0.15 g of the lead azide was weighed and added to 10 mL of distilled water, and the mixture was stirred to disperse the mixture evenly to obtain a lead azide dispersion; 0.002 g of pyrrole was added to 2.5 mL of ethanol to obtain a pyrrole dispersion; after the reaction container was mounted on the acoustic resonance platform, the reaction container was fixed, the resonance frequency was set to 63.8 Hz, the phase difference was set to 0.03, and the acceleration G1 was 60 g; the lead azide dispersion and the pyrrole dispersion were added to the reaction container, and the temperature of the reaction container was adjusted to 0°C; 0.10 g of sodium dodecylbenzene sulfonate was added to the reaction container, 2 mL of a FeCl3 solution with a concentration of 0.004 mol / mL was prepared, and the mixture was placed in an ice bath at 0°C; 0.5 mL of the FeCl3 solution was slowly added to the reaction container, and the mixed solution in the container was reacted at 0°C for 30 min, filtered, washed, and dried to obtain a core-shell structure composite material (LA / PPy composite material).

[0049] According to conversion rate = mass of reacting substance / total mass of reactants × 100%, the conversion rate is calculated to be 90%. Compared with the traditional paddle reaction, the product yield is higher. The electrostatic sensitivity of LA / PPy composite material is 1.25J, which is much higher than pure LA. Example

[0050] In this embodiment, first weigh 1.32g of sodium azide (NaN3) and dissolve it in 40mL of deionized water to obtain a sodium azide solution; weigh 1.65g of lead nitrate (Pb(NO3)2) and dissolve it in 40mL of deionized water, drop dilute nitric acid (concentration of 1%) to adjust the pH of the lead nitrate solution to 3 to obtain a lead nitrate solution; after the reaction container is installed on the acoustic resonance platform, the reaction container is fixed, the resonance frequency is set to 63.8Hz, the phase difference is set to 0.02, the acceleration G1 is 60g, and the above-configured lead nitrate solution and sodium azide solution are respectively added to the reaction container by a metering pump, the materials in the reaction container are reacted at room temperature for 1min, the temperature of the reaction system is raised to 65°C, and the reaction is continued at 65°C for 10min; after the reaction is completed, cool and filter, and the obtained lead azide The mixture was washed with deionized water and ethanol in turn, and dried in a vacuum drying oven to obtain a dry lead azide product; 0.20 g of the lead azide was weighed and added to 10 mL of distilled water, and the mixture was stirred to disperse evenly to obtain a lead azide dispersion; 0.002 g of pyrrole was added to 2.5 mL of ethanol to obtain a pyrrole dispersion, and the reaction container was mounted on an acoustic resonance platform, and the reaction container was fixed, the resonance frequency was set to 63.8 Hz, the phase difference was set to 0.03, and the acceleration G1 was 60 g. The lead azide dispersion and the pyrrole dispersion were added to the reaction container, and the temperature of the reaction container was adjusted to 0°C, 0.10 g of sodium dodecylbenzene sulfonate was added to the reaction container, 2 mL of a FeCl3 solution with a concentration of 0.004 mol / mL was prepared, and the mixture was placed in an ice bath at 0°C, 0.5 mL of the FeCl3 solution was measured and slowly added to the reaction container, and the mixed solution in the container was reacted at 0°C for 30 min, filtered, washed, and dried to obtain a core-shell structure composite material (LA / PPy composite material).

[0051] According to conversion rate = mass of reacting substance / total mass of reactants × 100%, the conversion rate is calculated to be 91%. Compared with the traditional paddle reaction, the product yield is higher. The electrostatic sensitivity of LA / PPy composite material is 1.1J, which is much higher than that of pure LA. Example

[0052] In this embodiment, first weigh 1.32g of sodium azide (NaN3) and dissolve it in 40mL of deionized water to obtain a sodium azide solution; weigh 1.65g of lead nitrate (Pb(NO3)2) and dissolve it in 40mL of deionized water, drop dilute nitric acid (concentration of 1%) to adjust the pH of the lead nitrate solution to 3 to obtain a lead nitrate solution; after the reaction container is installed on the acoustic resonance platform, the reaction container is fixed, the resonance frequency is set to 63.8Hz, the phase difference is set to 0.02, the acceleration G1 is 60g, and the above-configured lead nitrate solution and sodium azide solution are respectively added to the reaction container by a metering pump, the materials in the reaction container are reacted at room temperature for 1min, the temperature of the reaction system is raised to 65°C, and the reaction is continued at 65°C for 10min; after the reaction is completed, cool and filter, and the obtained lead azide The mixture was washed with deionized water and ethanol in turn, and dried in a vacuum drying oven to obtain a dry lead azide product; 0.10 g of the lead azide was weighed and added to 10 mL of distilled water, and the mixture was stirred to disperse the mixture evenly to obtain a lead azide dispersion; 0.002 g of pyrrole was added to 2.5 mL of ethanol to obtain a pyrrole dispersion; after the reaction container was mounted on the acoustic resonance platform, the reaction container was fixed, the resonance frequency was set to 63.8 Hz, the phase difference was set to 0.03, and the acceleration G1 was 60 g; the lead azide dispersion and the pyrrole dispersion were added to the reaction container, and the temperature of the reaction container was adjusted to 0°C; 0.10 g of sodium dodecylbenzene sulfonate was added to the reaction container, 2 mL of a FeCl3 solution with a concentration of 0.004 mol / mL was prepared, and the mixture was placed in an ice bath at 0°C; 0.5 mL of the FeCl3 solution was slowly added to the reaction container, and the mixed solution in the container was reacted at 0°C for 30 min, filtered, washed, and dried to obtain a core-shell structure composite material (LA / PPy composite material).

[0053] According to conversion rate = mass of reacting substance / total mass of reactants × 100%, the conversion rate is calculated to be 91%. Compared with the traditional paddle reaction, the product yield is higher. The electrostatic sensitivity of LA / PPy composite material is 1.3J, which is much higher than that of pure LA. Example

[0054] In this embodiment, first weigh 1.32g of sodium azide (NaN3) and dissolve it in 40mL of deionized water to obtain a sodium azide solution; weigh 1.65g of lead nitrate (Pb(NO3)2) and dissolve it in 40mL of deionized water, drop dilute nitric acid (concentration of 1%) to adjust the pH of the lead nitrate solution to 3 to obtain a lead nitrate solution; after the reaction container is installed on the acoustic resonance platform, the reaction container is fixed, the resonance frequency is set to 63.8Hz, the phase difference is set to 0.02, the acceleration G1 is 60g, and the above-configured lead nitrate solution and sodium azide solution are respectively added to the reaction container by a metering pump, the materials in the reaction container are reacted at room temperature for 1min, the temperature of the reaction system is raised to 65°C, and the reaction is continued at 65°C for 10min; after the reaction is completed, cool and filter, and the obtained lead azide The mixture was washed with deionized water and ethanol in turn, and dried in a vacuum drying oven to obtain a dry lead azide product; 0.15 g of the lead azide was weighed and added to 10 mL of distilled water, and the mixture was stirred to disperse the mixture evenly to obtain a lead azide dispersion; 0.002 g of pyrrole was added to 2.5 mL of ethanol to obtain a pyrrole dispersion; after the reaction container was mounted on the acoustic resonance platform, the reaction container was fixed, the resonance frequency was set to 63.8 Hz, the phase difference was set to 0.03, and the acceleration G1 was 60 g; the lead azide dispersion and the pyrrole dispersion were added to the reaction container, and the temperature of the reaction container was adjusted to 0°C; 0.10 g of sodium dodecylbenzene sulfonate was added to the reaction container, 2 mL of a FeCl3 solution with a concentration of 0.004 mol / mL was prepared, and the mixture was placed in an ice bath at 0°C; 0.5 mL of the FeCl3 solution was slowly added to the reaction container, and the mixed solution in the container was reacted at 0°C for 15 min, filtered, washed, and dried to obtain a core-shell structure composite material (LA / PPy composite material).

[0055] According to conversion rate = mass of reacting substance / total mass of reactants × 100%, the conversion rate is calculated to be 88%. Compared with the traditional paddle reaction, the product yield is higher. The electrostatic sensitivity of LA / PPy composite material is 1.25J, which is much higher than that of pure LA.

[0056] The substance concentrations and weights in the examples are only examples and should not be construed as limitations on the technical solutions of the present application.

[0057] The examples of the present application also describe a lead azide / conductive polymer, which is prepared using the lead azide / conductive polymer preparation method described in the previous examples.

[0058] The examples of the present application also describe a use of lead azide / conductive polymer. The lead azide / conductive polymer of the examples of the present application can be used as an explosive.

[0059] It should be understood that "one embodiment" or "an embodiment" mentioned throughout the specification means that specific features, structures or characteristics related to the embodiment are included in at least one embodiment of the present application. Therefore, "in one embodiment" or "in an embodiment" appearing throughout the specification does not necessarily refer to the same embodiment. In addition, these specific features, structures or characteristics can be combined in one or more embodiments in any suitable manner. It should be understood that in various embodiments of the present application, the size of the sequence number of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiment of the present application. The above-mentioned sequence numbers of the embodiments of the present application are for description only and do not represent the advantages and disadvantages of the embodiments.

[0060] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0061] The above is only an implementation method of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing lead azide / conductive polymer, It is characterized in that The method comprises: Preparing a lead nitrate solution of a first set concentration, dropping dilute nitric acid into it, and adjusting the pH value of the lead nitrate solution to a set value; preparing a sodium azide solution with a second set concentration; After installing the first reaction container on the first acoustic resonance platform, adjusting the resonance frequency and phase difference of the first acoustic resonance reaction platform so that the acceleration of the first acoustic resonance reaction platform is maintained within a first set range, and adding the lead nitrate solution and the sodium azide solution into the reaction container respectively; After reacting for a first set time, heating the first reaction container to a first set temperature, and then reacting for a second set time; After the reaction is completed, a suspension is obtained, the suspension is filtered to obtain a filtrate, the filtrate is washed with ethanol for multiple times, and then dried to obtain lead azide; Adding the prepared lead azide into an appropriate amount of distilled water, stirring and dispersing the lead azide evenly to obtain a lead azide dispersion, so that the lead azide in the lead azide dispersion reaches a third set concentration; adding pyrrole to an appropriate amount of ethanol to obtain a pyrrole dispersion, so that the pyrrole in the pyrrole dispersion reaches a fourth set concentration; After installing the second reaction container on the second acoustic resonance platform, adjusting the resonance frequency and phase difference of the second acoustic resonance reaction platform so that the acceleration of the second acoustic resonance reaction platform is maintained within a second set range, respectively adding the lead azide dispersion and the pyrrole dispersion into the second reaction container; heating the second reaction container to a second set temperature; wherein the volume ratio of the lead azide dispersion to the pyrrole dispersion is 24:7 to 21:5; Sodium dodecylbenzene sulfonate was added to the second reaction vessel, and the fifth set concentration of FeCl 3 The solution is slowly added into the second reaction container, and after the mixed solution in the second reaction container reacts at a third set temperature for a third set time, the reactant is filtered, washed, and dried to obtain a core-shell structure composite material, namely, a lead azide / PPy composite material; The mass ratio of the sodium dodecylbenzene sulfonate to the lead azide dispersion is 1:100 to 1:105, and the FeCl 3 The mass ratio of the solution to the lead azide dispersion is 1:24 to 1:

26.

2. The preparation method according to claim 1, It is characterized in that The first set concentration is: 0.02g / mL to 3g / mL; the second set concentration is: 0.05g / mL to 6g / mL; the third set concentration is: 0.9g / mL to 2.3g / mL; the fourth set concentration is: 0.06g / mL to 0.11g / mL; the fifth set concentration is: 0.0032mol / mL~0.0048mol / mL.

3. The preparation method according to claim 1, It is characterized in that The set value is 2.6~3.

2.

4. The preparation method according to claim 1, It is characterized in that The resonance frequency of the first acoustic resonance platform is 52-70 Hz; the phase difference of the first acoustic resonance platform ranges from 0.01 to 0.4; and the acceleration is maintained at 12 g to 185 g.

5. The preparation method according to claim 1, It is characterized in that The resonance frequency of the second acoustic resonance platform is 50-70 Hz; the phase difference of the second acoustic resonance platform ranges from 0.02 to 0.35; and the acceleration is maintained at 20 g to 175 g.

6. The preparation method according to claim 1, It is characterized in that The first set temperature is 25°C to 95°C; the second set temperature is 0°C to 2.5°C; and the third set temperature is 0°C to 1°C.

7. The preparation method according to claim 1, It is characterized in that The first set time length is 0.1min to 2min; the second set time length is 1min to 120min; and the third set time length is 1min to 60min.

8. The preparation method according to claim 1, It is characterized in that The content of PPy in the lead azide / PPy composite is 0.01 wt % to 16 wt %, and the content of lead azide is 84 wt % to 99.99 wt %.

9. A lead azide / conductive polymer, It is characterized in that The lead azide / conductive polymer is prepared by the lead azide / conductive polymer preparation method according to any one of claims 1 to 8.

10. Use of the lead azide / conductive polymer according to any one of claims 1 to 8, It is characterized in that The lead azide / conductive polymer is used as the primary explosive.