Preparation method of hydrogel flexible sensor based on ultrasonic carbon fiber patterning
The preparation method of hydrogel flexible sensors patterned by ultrasonic carbon fiber solves the problem of insufficient electrical sensing performance caused by low co-directional ratio of carbon fiber after stretching. It achieves high-resolution pattern arrangement and complex geometric shape construction, and improves the material quality. The biosafety and material compatibility ensure the stability and conductive properties of the material after large stretching.
Patent Information
- Application Number
- CN202410877341.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-02
AI Technical Summary
In the existing technology, the co-directional ratio of carbon fiber after stretching treatment is not high, which leads to the problem that the electrical sensing performance does not increase significantly.
A method for preparing a hydrogel flexible sensor patterned by ultrasonic carbon fiber is used. After configuring the hydrogel mixture and carbon fiber, an ultrasonic signal generator is used to arrange the carbon fiber in the mold to form a patterned arrangement, thereby improving the electrical properties and mechanics. performance.
A flexible sensor with no internal defects, good electrical properties, stable mechanical properties, and strong fatigue resistance has been realized. It can realize the arrangement of different patterns under certain boundary conditions. The material can still return to its original shape after large stretching, and the resistance value changes stably. , has good flexibility and ductility.
Smart Images

Figure CN118755015A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technology in the field of flexible sensors, in particular to a method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning. Background Art
[0002] With the development of wearable electronic devices, smart medical care, electronic skin and other fields, flexible sensors have been widely studied and applied as a key technology. They have the advantages of wide application range, high sensitivity, flexible and convenient operation, and strong anti-interference ability. At present, flexible sensors based on conductive particle-hydrogel-based composites have attracted widespread attention due to their large tensile strain range, high flexibility and relatively stable dynamic characteristics. Among various conductive fillers that enhance the electromechanical properties of materials (such as carbon fiber, silver powder, graphene, etc.), carbon fiber is increasingly used as a conductive reinforcement material to improve the sensing performance of original polymer composites due to its high strength, high modulus, low density, good thermal conductivity and electrical conductivity, and low price. Summary of the invention
[0003] In view of the problem in the prior art that the isotropic rate of carbon fibers after stretching treatment is not high, and some carbon fibers still maintain different angles with the stretching direction, resulting in a lack of obvious increase in electrical sensing performance, the present invention proposes a method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning. The ultrasonic manipulation technology has the characteristics of high material compatibility, non-invasiveness and no labels. The prepared flexible sensor has no internal defects, good electrical properties, stable mechanical properties, strong fatigue resistance, and can achieve the arrangement of different patterns under certain boundary conditions.
[0004] The present invention is achieved through the following technical solutions:
[0005] The present invention relates to a method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning. The method comprises the following steps: preparing a hydrogel mixed liquid, adding carbon fibers and dispersing the mixed liquid evenly, pouring the mixed liquid into a mold, and ultrasonically arranging the carbon fibers in the mold through an external ultrasonic signal generator. Finally, the mixed liquid is cured to obtain a hydrogel-based composite material having patterned carbon fibers.
[0006] The hydrogel mixture is a mixture of N,N-dimethylacrylamide (DMAA) and 2-acrylamide-2-methyl-1-propane sulfonic acid (AMPS), specifically refers to a mixture of DMAA, a photoinitiator, polyethylene glycol, a diacrylate and an aqueous solution of AMPS, wherein the mass ratio of N,N-dimethylacrylamide (DMAA) to 2-acrylamide-2-methyl-1-propane sulfonic acid (AMPS) is preferably 1:3-3:1, and more preferably 2:1.
[0007] The carbon fiber is preferably 350 microns in length and 50 microns in diameter.
[0008] The hydrogel mixture is preferably stored in a sealed light-proof container after being fully mixed.
[0009] The sufficient mixing is achieved by, but not limited to, ultrasonic dispersion, specifically by ultrasonically oscillating in a sealed, light-proof container for more than 30 minutes.
[0010] The mass fraction of the carbon fiber and hydrogel mixture is 0.5%-5%. When the mass fraction is less than 0.5%, the carbon fiber concentration is too low and the electrical sensing performance is not significantly improved; when the mass fraction is greater than 5%, the carbon fiber concentration is too high and an effective linear arrangement cannot be formed.
[0011] The uniform dispersion is achieved by, but not limited to, ultrasonic dispersion, specifically by ultrasonically oscillating in a sealed, light-proof container for more than 30 minutes.
[0012] The mold is a rectangular parallelepiped structure, and a side edge of the top surface of the mold is provided with a groove without side walls. The side wall-free structure facilitates the piezoelectric transducer to directly contact the solution, thereby forming a more obvious excitation effect on the particles and enhancing the arrangement effect.
[0013] The sidewall-free groove preferably has a depth of 200-500 microns, a length of 20 millimeters, and a width of 5 millimeters.
[0014] The mold is preferably printed by a light-curing 3D printer, and the mold is rinsed with anhydrous ethanol and dried. The piezoelectric transducer is pasted to the side without the sidewall groove for demoulding, and then left to dry.
[0015] The ultrasonic signal generator comprises a signal generator and a power amplifier.
[0016] The ultrasonic arrangement is achieved by adjusting the frequency of the signal generator to the optimal frequency of the piezoelectric transducer and adjusting the amplitude to within 2Vpp; connecting the signal generator to a power amplifier and setting the magnification to 8-10 times; and connecting the power amplifier to the piezoelectric transducer. When the power amplification exceeds 10 times, the piezoelectric transducer will generate heat, which will easily evaporate the water in the solution in the cavity and affect the preparation effect. When the power amplification exceeds the low level, the piezoelectric transducer cannot generate an effective sound field to drive the particle arrangement.
[0017] The ultrasonic arrangement lasts for about 10 seconds. If the arrangement time is too long, it will cause degumming, particle agglomeration and other phenomena.
[0018] The curing refers to curing the sample with a 405 nm wavelength UV lamp, which is preferably fixed 20 cm above the surface of the groove of the hydrogel solution containing carbon fibers, and irradiated for 3-10 seconds, preferably 3s-5s.
[0019] The present invention relates to the application of the hydrogel-based composite material prepared by the method, which is encapsulated together with a conductive medium in a waterproof material to form a resistive sensor. Technical Effects
[0020] The present invention uses an ultrasonic method to disperse and arrange the carbon fiber in the hydrogel solution, thereby ensuring the dispersibility of the carbon fiber. Compared with the prior art, the present invention can design the arrangement of the particles in the solution according to the actual situation with a high-resolution pattern, construct a complex geometric shape, have good ultrasonic penetration, high biosafety and material compatibility, require less raw materials for particles, and have a simple operation process. Under the action of external force, stress or strain changes are generated, and the resistance value of the material changes greatly; the stability is high, and the material can still restore the original length of the material in a short time when the stretching amount reaches 5 times the original length, and the resistance value and the resistance value change tend to be stable; the stretchability is strong, with good flexibility and ductility, the material still has basic conductive properties after the stretching amount is greater than 600%, and the material itself does not have obvious damage cracks and gaps; the fatigue resistance is strong and the repeatability is good. In more than 100 repeated pullings, the resistance value tends to be stable, the material shape changes less, and the sample has no permanent deformation. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a flow chart of the present invention;
[0022] Figure 2 This is a schematic diagram of ultrasound arrangement;
[0023] Figure 3 This is the effect picture of carbon fiber reinforced hydrogel after ultrasonic arrangement;
[0024] Figure 4 Schematic diagram of carbon fiber reinforced hydrogel flexible sensor;
[0025] In the figure: pure copper conductor 1, VHB tape 2, hydrogel-based composite material 3 prepared by the present invention;
[0026] Figure 5 This is a graph showing the fatigue resistance of carbon fiber reinforced hydrogel;
[0027] Figure 6 Electrical performance diagram of carbon fiber reinforced hydrogel flexible sensor. DETAILED DESCRIPTION
[0028] like Figure 1 As shown, this embodiment relates to a method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning, comprising:
[0029] Step a, weighing 5g N,N-dimethylacrylamide (DMAA), 0.2g photoinitiator (TPO-L), and 0.02g polyethylene glycol (400) diacrylate (PEG400DA), adding them to a 50ml sealed light-proof bottle and shaking them well, ultrasonically oscillating them at room temperature for 30 minutes to mix the components evenly, and obtaining liquid A; weighing 5g 2-acrylamido-2-methyl-1-propane sulfonic acid (AMPS) and 5g pure water, adding them to a 50ml sealed light-proof bottle and shaking them well, ultrasonically oscillating them at room temperature for 30 minutes to mix the components evenly, and obtaining liquid B; mixing the prepared liquid A and liquid B in a ratio of 2:1, ultrasonically oscillating them at room temperature and light-proof environment for 30 minutes to fully mix them, and obtaining a hydrogel solution C;
[0030] Step b, weighing carbon fibers with a length of 350 microns, and adding the hydrogel solution C at a mass concentration of 0 to 10% to obtain a mixture D;
[0031] Step c, placing the mixed solution D in a room temperature, dark environment, and ultrasonically vibrating for 1 hour to make the carbon fibers evenly distributed in the solution;
[0032] Step d, using CAD software to design a mold with a length of 20 millimeters (mm), a width of 5 millimeters (mm), and a depth of 200 to 500 microns (um), and using a light-curing 3D printer to prepare the mold;
[0033] Step e, soaking the printed mold in anhydrous ethanol solution for a period of time to ensure that there is no resin residue on the surface;
[0034] Step f, taking out the mold and placing it in a hot oven at 50°C for 20 minutes for drying;
[0035] Step g, using an electric welding gun to apply solder to the positive and negative electrodes of the piezoelectric transducer, and welding the wires to the positive and negative electrodes; taking out the pretreated mold, applying ultrasonic coupling agent to the surface without side walls, and pasting the piezoelectric transducer to the surface without side walls;
[0036] Step h, placing the mold for pasting the piezoelectric transducer in a fume hood, spraying an aerosol release agent evenly at a distance of 20 cm from the mold, and letting it stand to dry;
[0037] Step i: Turn on the signal generator, adjust the parameters to the optimal frequency of the piezoelectric transducer of 1.8MHz, and arrange the optimal amplitude of 1.8Vpp; connect the signal generator to the power amplifier and set the magnification to 10 times; take out the mold that has been demoulded in step h), connect the positive and negative electrodes to the power amplifier, and place them at the observation point directly below the microscope. Take out the solution in step c), and drop the liquid into the groove with a dropper;
[0038] Step j, adjusting the microscope light and focal length to the optimal imaging state, turning on the signal generating device, and observing the movement of particles inside the groove through the microscope;
[0039] Step k, after observing that the particles are arranged in an ideal linear manner, irradiate the solution into a thin sheet by using an LED ultraviolet UV curing lamp with a wavelength of 365 nm at a height of about 20 cm above the mold for 10 to 30 seconds, and take out the solidified thin sheet in the groove to obtain a composite material formed by the arrangement of carbon fibers in the hydrogel;
[0040] like Figure 2 As shown, the ultrasonic arrangement uses sound waves to drive the carbon fiber particles evenly dispersed in the hydrogel solution in the groove, forming an ultrasonic energy field in the specified groove area, and through the acoustic standing wave, the particles in the hydrogel solution are affected by the acoustic radiation force to move in the propagation direction of the ultrasonic energy field and finally remain stable in the trough area of the ultrasonic standing wave.
[0041] like Figure 3 As shown in the figure, it is the actual effect after ultrasonic arrangement of this embodiment. According to the natural frequency of the piezoelectric transducer, the output signal frequency of the signal generator is adjusted to generate stripe patterns with different spacings. During the experiment, piezoelectric transducers with natural frequencies of 1 MHz, 1.8 MHz, and 3 MHz are used to form patterned arrangements of lines with different spacings.
[0042] like Figure 4 As shown, this is the application of the carbon fiber reinforced hydrogel flexible material prepared by the above method in this embodiment. The hydrogel-based composite material 3 and the pure copper wire 1 as a conductive medium are packaged in a VHB tape 2 to form a resistive sensor.
[0043] like Figure 5 As shown in FIG. 1 , the resistance response diagram of the resistive sensor of this embodiment at different stages when the resistive sensor is repeatedly stretched 100 times without pre-stretching amount. In the 100 cycles of driving, the sensor maintains a consistent response resistance size. It can be seen that the size of the sensor after repeated stretching does not change and there is no permanent deformation;
[0044] like Figure 6 As shown in FIG. 1 , the electrical performance diagram of the resistive sensor of this embodiment is shown in FIG. Figure 5 It can be seen that the sensitivity coefficient GF (strain gauge sensitivity coefficient) of the flexible sensor prepared after ultrasonic arrangement treatment of carbon fiber in hydrogel solution, that is, the measured value of resistance change per strain, is significantly better than the sensitivity coefficient of pure hydrogel and carbon powder hydrogel solution.
[0045] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.
Claims
1. A method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning, characterized in that: A hydrogel mixed solution is prepared and carbon fibers are added and dispersed uniformly, then poured into a mold and the carbon fibers in the mold are ultrasonically arranged by an external ultrasonic signal generator, and finally cured to obtain a hydrogel-based composite material with patterned carbon fibers; The hydrogel mixture is a mixture of N,N-dimethylacrylamide (DMAA) and 2-acrylamido-2-methyl-1-propanesulfonic acid (AMPS); The uniform dispersion is achieved by ultrasonic dispersion.
2. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1 is characterized in that: The hydrogel mixture is a mixture of DMAA, a photoinitiator, polyethylene glycol, a diacrylate and an aqueous solution of AMPS, wherein the mass ratio of N,N-dimethylacrylamide (DMAA) to 2-acrylamido-2-methyl-1-propanesulfonic acid (AMPS) is 1:3-3:
1.
3. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1 or 2, characterized in that: The mass ratio of the N,N-dimethylacrylamide (DMAA) to 2-acrylamido-2-methyl-1-propanesulfonic acid (AMPS) is 2:
1.
4. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1, characterized in that: The carbon fiber has a length of 350 microns and a diameter of 50 microns.
5. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1, characterized in that: The ultrasonic dispersion is specifically: ultrasonically vibrating in a sealed light-proof container for more than 30 minutes.
6. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1 or 3, characterized in that: The mass fraction of the carbon fiber and hydrogel mixed liquid is 0.5%-5%.
7. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1, characterized in that: The mold is a rectangular parallelepiped structure, and a side edge of the top surface of the mold is provided with a groove without side walls. The side wall-free structure facilitates the piezoelectric transducer to directly contact the solution, thereby forming a more obvious excitation effect on the particles and enhancing the arrangement effect.
8. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1, characterized in that: The ultrasonic arrangement is achieved by adjusting the frequency of the signal generator to the optimal frequency of the piezoelectric transducer and adjusting the amplitude to within 2Vpp; the signal generator is connected to a power amplifier and the amplification factor is set to 8-10 times.
9. The method for preparing a hydrogel flexible sensor based on ultrasonic carbon fiber patterning according to claim 1, characterized in that: The curing refers to curing the sample using a UV lamp with a wavelength of 405 nm.
10. An application of a hydrogel-based composite material prepared by the method according to any one of claims 1 to 9, characterized in that: It is encapsulated together with the conductive medium in a waterproof material to form a resistive sensor.
Citation Information
Patent Citations
Method for producing carbon nanotube fiber aggregate having improved level of alignment
CN109563648A
Conductive hydrogel
JP2018070894A
A Piezoelectric Paper Fabrication Using An Ultrasonic Wave Ion Removal Technique
KR1020120057106A
Method for manufacturing flexible sensor
US20230340225A1
Method of reordering fibres in a web
US4119447A