Preparation method of filler for electromagnetic shielding film, filler and electromagnetic shielding film
Through the synergistic effect of carbon fiber and metal particles, combined with thermoplastic resin, an electromagnetic shielding film that is lightweight, has good conductivity, and is easy to process is prepared, which solves the problems of heavy weight and poor corrosion resistance of existing electromagnetic shielding materials and achieves efficient electromagnetic shielding. Performance and applicability.
Patent Information
- Application Number
- CN202410982398.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
AI Technical Summary
Existing electromagnetic shielding materials are heavy, have poor corrosion resistance, and have high rigidity, making it difficult to meet the needs of light weight, small size, and foldability. In addition, high filling amounts lead to high costs, difficult processing, and poor transparency, making it difficult to meet the needs of various applications. .
Modified carbon fiber is prepared by reacting carbon fiber with a pore-forming agent. Air is removed through nitrogen replacement. The temperature is raised to react between the pore-forming agent and the carbon fiber. Then the temperature is lowered and ground to form a pore structure. Then it is heated in a metal salt solution to react metal ions with the modified carbon fiber. , form metal particles, prepare the filler of the electromagnetic shielding film, and combine with thermoplastic resin to prepare the electromagnetic shielding film through twin-screw extrusion and stretching processes.
An electromagnetic shielding film that is light in weight, has excellent conductivity and is easy to process has been realized. It has good electromagnetic shielding performance and is suitable for a variety of electronic components. The process is simple, solvent-free and suitable for mass production.
Smart Images

Figure BDA0004957545820000091 
Figure BDA0004957545820000101
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of carbon fiber composite materials, and specifically relates to a preparation method of a filler for an electromagnetic shielding film, the filler and the electromagnetic shielding film. Background Art
[0002] Electromagnetic interference is a type of electronic interference generated by electromagnetic waves. It can originate from natural phenomena such as solar flares, lightning, and electrostatic discharge, or it can be generated by electronic devices. In recent years, due to the development of science and technology and the orientation of human needs, electronic devices have developed in the direction of being smaller, lighter, and more reliable, which requires portable electronic devices to have higher power and faster operating speeds. However, when electronic devices are running at high power and high speed, they will radiate a large amount of high-frequency electromagnetic waves, such as microwaves and radio frequency electromagnetic waves. These electromagnetic waves will not only interrupt or hinder the effective operation of neighboring equipment, but more seriously, they will pollute the ecological environment and endanger the health of organisms. At present, in the civil and military fields, the use of electromagnetic shielding technology is one of the most effective ways to protect the natural environment from electromagnetic pollution, equipment from electromagnetic interference, and surrounding organisms from electromagnetic hazards.
[0003] The electromagnetic shielding materials that have been developed include metals and metal oxides, transition metal carbides / nitrides, carbon-based materials and conductive polymer materials. The metal and metal oxide materials that have been studied the longest and are the most widely used have disadvantages such as heavy weight, poor corrosion resistance and high rigidity, which make it difficult to meet the current requirements for electromagnetic shielding materials such as light weight, small size and foldability.
[0004] For example, Chinese patent CN110767075A discloses a flexible anti-counterfeiting layer based on a metal micro-nano network, its preparation method and use. The preparation method of the anti-counterfeiting layer includes the following steps: preparing a metal material, patterning the metal material to obtain a metal network with a specific pattern, i.e., a patterned metal network; transferring the obtained patterned metal network to a product that needs to be anti-counterfeited, to obtain a flexible anti-counterfeiting layer of a metal micro-nano network. The metal network of this technical solution has a regular grid shape and is prepared by an etching method. The obtained anti-counterfeiting layer has low environmental weather resistance, adhesion and shielding effectiveness.
[0005] Another example is the electromagnetic shielding film of Chinese patent CN113853839A, which uses a conductive adhesive layer containing conductive particles and a bonding resin composition. The filling amount of the conductive filler needs to reach above its percolation threshold to have conductivity and electromagnetic shielding performance, and the higher the filling amount, the better the electromagnetic shielding effect of the shielding film, but the adhesion is weakened. A higher filling amount will undoubtedly bring high cost, high weight and difficult processing. In addition, it is difficult for the filled electromagnetic shielding film to obtain the characteristic of being transparent to visible light, which limits its use in certain specific occasions.
[0006] For this purpose, an electromagnetic shielding film which is light in weight, has strong electromagnetic shielding properties and is easy to process is needed. Summary of the invention
[0007] The object of the present invention is to provide an improved method for preparing a filler for an electromagnetic shielding film, the filler and the electromagnetic shielding film.
[0008] In order to achieve the above object, a technical solution adopted by the present invention is:
[0009] A method for preparing a filler for an electromagnetic shielding film, comprising:
[0010] S1, placing carbon fiber and pore-forming agent in a reactor, replacing the air in the reactor with nitrogen, raising the temperature to allow the pore-forming agent to react with the carbon fiber, then cooling and grinding to obtain modified carbon fiber;
[0011] S2, adding the modified carbon fiber of step S1 and a surfactant to the metal salt solution, heating to remove the solvent and then grinding to obtain a powder;
[0012] S3, placing the powder of step S2 in a reactor, replacing the air in the reactor with nitrogen, heating the reactor so that the metal ions react with the modified carbon fibers, then cooling and grinding to obtain the filler.
[0013] In step S1, the carbon fiber is mainly composed of carbon element, which is light in weight, good in chemical stability and excellent in electrical conductivity. The carbon fiber can be carbon fiber powder, carbon fiber short fiber, carbon fiber long fiber, carbon fiber filament, carbon fiber cloth, etc. In order to facilitate grinding to prepare fillers with smaller particle size, the carbon fiber is preferably carbon fiber powder.
[0014] The pore-forming agent can decompose at high temperature to produce a large amount of gas, and can create a large number of pores on the carbon fiber, such as macropores, mesopores, micropores, etc. The modified carbon fiber that is easy to prepare can better absorb the metal salt solution and improve the dispersion of the metal particles after high-temperature treatment. The pores on the carbon fiber are regulated by adjusting the mass ratio of the carbon fiber and the pore-forming agent. After having a developed pore structure, more and more dispersed metal salts can be adsorbed, and uniform metal particles can be formed in the subsequent high-temperature roasting, and metal-C bonds can also be formed.
[0015] In some embodiments, in step S1, the pore-forming agent is one or more of potassium hydroxide, potassium carbonate, potassium bicarbonate, potassium nitrate, sodium carbonate, sodium bicarbonate, zinc chloride, and zinc nitrate. For better porosity, the pore-forming agent is preferably one or more of potassium carbonate and potassium hydroxide.
[0016] In some embodiments, in step S1, in order to obtain a better porosity, the mass ratio of the carbon fiber to the pore-forming agent is 1:0.1 to 1:0.9. If the amount of pore-forming agent is small, the porosity is insufficient, which may lead to poor metal dispersion and reduced electromagnetic shielding capability; if the amount is large, the pores are developed, the metal salt is adsorbed more, and metal sintering is easy to occur, the metal particles are large, and the metal utilization rate is not high. The mass ratio of carbon fiber to pore-forming agent is preferably 1:0.3 to 1:0.7.
[0017] In some embodiments, in step S1, the average particle size of the modified carbon fiber is 10 to 100 μm.
[0018] In some embodiments, in step S1, after nitrogen replacement, the temperature is raised to 800-1200° C., kept for 2-5 hours, cooled to room temperature, and ground and sieved to obtain the modified carbon fiber.
[0019] In some embodiments, in step S2, the metal salt solution is prepared by mixing the metal salt with the solvent and stirring for a certain period of time to obtain the metal salt solution, wherein the conductivity of the metal salt corresponding to the metal element is greater than or equal to 1.0×10 6 S / m.
[0020] In some embodiments, the metal in the metal salt solution includes a combination of one or more of iron, cobalt, nickel, copper, zinc, aluminum, titanium, vanadium, chromium, manganese, silver, platinum, and gold. The metal salt and the modified carbon fiber can form metal particles after high temperature, and the synergistic effect with the carbon fiber is conducive to the formation of an electromagnetic shielding film with better electromagnetic shielding performance. If it is copper chloride, copper ions participate in the reaction, and finally form metal particles in the subsequent high-temperature roasting, and the obtained metal particles are single copper.
[0021] In step S2, a solvent is used to dissolve the metal salt to form a uniform solution, which is convenient for the modified carbon fiber to adsorb the metal salt. The solvent is a combination of one or more of water, methanol, ethanol, ethyl acetate, dichloromethane, and ethylene glycol. For cost control, one or more of water or ethanol is preferred.
[0022] In some embodiments, if the amount of metal salt used is small, the shielding effectiveness of the prepared film is reduced; if the amount of metal salt used is large, it is easy to cause metal agglomeration and sintering, reducing the metal utilization rate. At the same time, considering the optimal metal particle loading rate and controlling the solvent evaporation rate, the mass ratio of the metal salt to the solvent is 0.05:1~0.2~1.
[0023] In order to obtain better electromagnetic shielding performance, the conductivity of the metal salt corresponding to the metal element is 1.0×10 6The conductivity is a parameter of the ease of charge flow in a substance. The larger the conductivity value, the faster the charge transfer of the substance, and the faster the reflection or absorption of electromagnetic waves. The copper salt is more preferably copper nitrate or copper chloride.
[0024] In some embodiments, modified carbon fiber and surfactant are added to a metal salt solution, the temperature is raised to 60-100° C., the solvent is removed by stirring in the open air, and the powder is obtained by grinding.
[0025] In step S2, the surfactant is used to disperse the metal salt solution and provide polar functional groups to bond the components and improve the overall mechanical properties.
[0026] In some embodiments, in step S2, the surfactant is a combination of one or more of fatty acid glycerides, fatty acid sorbitan, polyoxyethylene fatty acid esters, polyoxyethylene fatty alcohol ethers, polyvinyl pyrrolidone, and cetyl trimethyl ammonium bromide; preferably one or more of polyvinyl pyrrolidone and cetyl trimethyl ammonium bromide.
[0027] In some embodiments, in step S2, the mass ratio of the modified carbon fiber to the surfactant is 1:20:0.5 to 1:5:2.
[0028] In some embodiments, in step S2, when the mass ratio of metal salt solution: modified carbon fiber: surfactant is (1:20:0.5) to (1:5:2), the best shielding performance is achieved.
[0029] In some embodiments, in order to better adsorb the metal salt, the average particle size of the obtained modified carbon fiber is 10 to 100 μm, and more preferably 30 to 70 μm.
[0030] In order to mix evenly with the thermoplastic resin and facilitate the preparation of the film, in step S3, the average particle size of the filler prepared is 10 to 100 μm.
[0031] In some embodiments, in step S3, after nitrogen replacement, the temperature is raised to 400-800° C., kept for 1-3 hours, cooled to room temperature, and ground to obtain the filler.
[0032] Another technical solution adopted by the present invention is:
[0033] A filler prepared according to the method for preparing a filler for an electromagnetic shielding film.
[0034] Another technical solution adopted by the present invention is:
[0035] An electromagnetic shielding film comprises the filler for the electromagnetic shielding film and a thermoplastic resin. In parts by weight, the raw materials of the electromagnetic shielding film comprise: 100 parts of the thermoplastic resin; and 10 to 30 parts of the filler.
[0036] In some embodiments, if the amount of filler is small, the electromagnetic shielding performance of the electromagnetic shielding film is reduced. If the amount of filler is large and reaches the electromagnetic shielding threshold, the electromagnetic shielding capability is less improved. The amount of filler is preferably 15 to 25 parts by weight.
[0037] In some embodiments, the thermoplastic resin includes one or more combinations of polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyamide, polyoxymethylene, polycarbonate, polyphenylene oxide, polysulfone, rubber, polyethylene terephthalate, and polyethylene furandicarboxylate. Considering the strength of the base resin, one or more of polyethylene terephthalate and polyethylene furandicarboxylate are preferred.
[0038] Furthermore, the thermoplastic resin is in powder form, and the particle size of the thermoplastic resin is 10 to 100 μm.
[0039] The electromagnetic shielding film of the present invention can be prepared by the following method: placing the thermoplastic resin and filler in a high-speed stirrer, stirring for 20-60 minutes, and then extruding through a twin-screw extruder at an extrusion temperature of 200-300°C, subjecting the obtained product to a sheet casting process to obtain a pretreated sheet, and then subjecting the pretreated sheet to longitudinal and transverse stretching at a stretching temperature of 100-150°C, and transverse and longitudinal stretching ratios of 2-5 to obtain an electromagnetic shielding film.
[0040] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0041] The filler for electromagnetic shielding film provided by the present invention has carbon fiber and metal particles working together to have better conductivity; the filler realizes nano-scale dispersion of metal and compound carbon fiber; the preparation process of the electromagnetic shielding film of the present invention is solvent-free and simple; the electromagnetic shielding film of the present invention has electromagnetic shielding due to the dual effects of carbon fiber and metal, and has better electromagnetic shielding performance; the electromagnetic shielding film of the present invention is suitable for a variety of electronic components. DETAILED DESCRIPTION
[0042] The present invention is further described below in conjunction with the illustrated embodiments.
[0043] For electromagnetic shielding films, Examples 1-17 and Comparative Examples 1-6 are provided. The raw materials used in the Examples and Comparative Examples are as follows:
[0044]
Thermoplastic resin
[0045] A1: Polyethylene terephthalate, Sinopec Polyethylene terephthalate FG600;
[0046] A2: Poly(ethylene furandicarboxylate), Poly(ethylene furandicarboxylate) resin produced by China Science and Technology Corporation.
[0047]
Carbon fiber
[0048] [Surfactant] Polyvinylpyrrolidone, brand P110608, produced by Aladdin (Shanghai) Reagent Co., Ltd.
[0049]
Filling material
[0050] B1:
[0051] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0052] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, and then fully grind, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0053] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0054] B2:
[0055] S1. Weigh a certain amount of carbon fiber and potassium carbonate in a reactor, the mass ratio of carbon fiber to potassium carbonate is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0056] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, and then fully grind, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0057] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0058] B3:
[0059] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0060] S2. Weigh copper chloride and water to prepare a uniform solution, wherein the mass ratio of copper chloride to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, and then fully grind, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0061] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0062] B4:
[0063] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0064] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and hexadecyltrimethylammonium bromide in a ratio of uniform solution: modified carbon fiber: hexadecyltrimethylammonium bromide = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0065] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0066] B5:
[0067] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 100 mesh sieve (147 μm) to obtain modified carbon fiber;
[0068] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 100 mesh sieve (147 μm) to obtain a powder;
[0069] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 100-mesh sieve (147 μm), and obtain filler.
[0070] B6:
[0071] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.1, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0072] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0073] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0074] B7:
[0075] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.9, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0076] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0077] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0078] B8:
[0079] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0080] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.05:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0081] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0082] B9:
[0083] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0084] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.2:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:10:1, place the three in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0085] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0086] B10:
[0087] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0088] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:20:0.5, place the three in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0089] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0090] B11:
[0091] S1. Weigh a certain amount of carbon fiber and potassium hydroxide in a reaction kettle, the mass ratio of carbon fiber to potassium hydroxide is 1:0.5, after nitrogen replacement, heat to 1000°C, stay for 3 hours, cool to room temperature, grind, and sieve through a 200 mesh sieve (75 μm) to obtain modified carbon fiber;
[0092] S2. Weigh copper nitrate and water to prepare a uniform solution, wherein the mass ratio of copper nitrate to water is 0.1:1; weigh the uniform solution, modified carbon fiber, and polyvinyl pyrrolidone, wherein the ratio is uniform solution: modified carbon fiber: polyvinyl pyrrolidone = 1:5:2, place the three in a beaker, stir and heat to 90°C, remove the solvent water, grind thoroughly, and sieve through a 200-mesh sieve (75 μm) to obtain a powder;
[0093] S3. Put the powder into a reactor, replace with nitrogen, heat to 600°C, stay for 2 hours, cool to room temperature, grind into powder, sieve with a 200-mesh sieve (75 μm), and obtain filler.
[0094] B12:
[0095] The difference from B1 is that there is no surfactant in step S2.
[0096] B13:
[0097] The difference from B1 is that there are no steps S2 and S3.
[0098] B14:
[0099] The difference from B1 is that there is no step S3.
[0100] B15:
[0101] The difference from B1 is that there are only carbon fibers in step S1.
[0102] B16:
[0103] Only metal salts are included.
[0104] B17:
[0105] The difference from B1 is that the mass ratio of carbon fiber to potassium hydroxide is 1:0.3.
[0106] B18:
[0107] The difference from B1 is that the mass ratio of carbon fiber to potassium hydroxide is 1:0.7.
[0108] Based on the above-mentioned thermoplastic resin and filler, an electromagnetic shielding film is prepared, and the method includes: placing the thermoplastic resin and filler in a high-speed stirrer, stirring for 30 minutes, and then extruding through a twin-screw at an extrusion temperature of 200-300°C, subjecting the obtained product to a casting process to obtain a pretreated sheet, and then longitudinally stretching and transversely stretching the pretreated sheet at a stretching temperature of 100-150°C, and the transverse and longitudinal stretching ratios are both 2-5 to obtain an electromagnetic shielding film.
[0109] The raw material formulas of Examples 1-17 and Comparative Examples 1-6 are shown in Table 1.
[0110] Table 1 Raw material formula of Examples 1-17 and Comparative Examples 1-6
[0111]
[0112] The electromagnetic shielding films of Examples 1-17 and Comparative Examples 1-6 were subjected to the following tests. Unless otherwise specified, each test was conducted at 25° C. The main indicators are as follows:
[0113] 1. Average electromagnetic shielding effectiveness: tested in accordance with GB / T30142-2013 standard;
[0114] 2. Tensile strength: tested according to GB / T 1040.1-2018;
[0115] 3. Elongation at break: Tested according to GB / T 1040-92.
[0116] The performance data of the electromagnetic shielding films of Examples 1-17 and Comparative Examples 1-6 are shown in Table 2.
[0117] Table 2 Performance data of electromagnetic shielding films of Examples 1-17 and Comparative Examples 1-6
[0118]
[0119] As shown in Tables 1 and 2, compared with Comparative Example 1-6, the electromagnetic shielding film prepared in Example 1-17 has better electromagnetic shielding effectiveness and superior mechanical properties; the preparation process of the electromagnetic shielding film prepared in Example 1-17 is simple and convenient, the preparation process is pollution-free, and it is easy to mass produce.
[0120] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a filler for an electromagnetic shielding film, characterized in that: include: S1, placing carbon fiber and pore-forming agent in a reaction kettle, replacing with nitrogen, heating, cooling and grinding to obtain modified carbon fiber; S2, adding the modified carbon fiber of step S1 to the metal salt solution, heating to remove the solvent and then grinding to obtain powder; S3, placing the powder from step S2 in a reaction kettle, replacing the atmosphere with nitrogen, heating, cooling, and grinding to obtain the filler.
2. The method for preparing a filler for an electromagnetic shielding film according to claim 1, characterized in that: In step S2, the metal salt solution is prepared by mixing a metal salt with a solvent to obtain a metal salt solution, wherein the metal in the metal salt solution includes a combination of one or more of iron, cobalt, nickel, copper, zinc, aluminum, titanium, vanadium, chromium, manganese, silver, platinum, and gold, and the solvent is a combination of one or more of water, methanol, ethanol, ethyl acetate, dichloromethane, and ethylene glycol.
3. The method for preparing a filler for an electromagnetic shielding film according to claim 2, characterized in that: The electrical conductivity of the metal salt corresponding to the metal element is greater than or equal to 1.0×10 6 S / m.
4. The method for preparing a filler for an electromagnetic shielding film according to claim 3, characterized in that: The mass ratio of the metal salt to the solvent is 0.05:1-0.2-1.
5. The method for preparing a filler for an electromagnetic shielding film according to claim 1, characterized in that: In step S2, the modified carbon fiber and surfactant of step S1 are added to the metal salt solution, wherein the surfactant is a combination of one or more of fatty acid glyceride, fatty acid sorbitan, polyoxyethylene fatty acid ester, polyoxyethylene fatty alcohol ether, polyvinyl pyrrolidone, and hexadecyltrimethylammonium bromide; and the mass ratio of the modified carbon fiber to the surfactant is 1:20:0.5 to 1:5:
2.
6. The method for preparing a filler for an electromagnetic shielding film according to claim 1, characterized in that: In step S1, the pore-forming agent is one or more of potassium hydroxide, potassium carbonate, potassium bicarbonate, potassium nitrate, sodium carbonate, sodium bicarbonate, zinc chloride, and zinc nitrate.
7. The method for preparing a filler for an electromagnetic shielding film according to claim 1, characterized in that: In step S1, the mass ratio of the carbon fiber to the pore-forming agent is 1:0.1 to 1:0.9; and\or in step S1, the average particle size of the modified carbon fiber is 10 to 100 μm; and\or in step S3, the average particle size of the prepared filler is 10 to 100 μm.
8. A filler prepared according to the method for preparing a filler for electromagnetic shielding film according to any one of claims 1 to 7.
9. An electromagnetic shielding film, characterized in that: Comprising the filler as claimed in claim 8 and a thermoplastic resin, the raw materials of the electromagnetic shielding film include, in parts by weight: 100 parts of thermoplastic resin; 10 to 30 parts of filler.
10. The electromagnetic shielding film according to claim 9, characterized in that The thermoplastic resin includes one or more of polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyamide, polyoxymethylene, polycarbonate, polyphenylene ether, polysulfone, rubber, polyethylene terephthalate, and polyethylene furandicarboxylate.