Waterproof organic silicon leather composite material and preparation method thereof

By using components such as MQ silicone resin, modified organic montmorillonite-silica composite materials, and new intercalating agents in silicone leather, the problem of insufficient waterproofness and antifouling properties of silicone leather has been solved, and high efficiency has been achieved. The waterproof and anti-fouling properties improve the durability and safety of leather.

CN118755269AInactive Publication Date: 2024-10-11JIANGZHI (GUANGDONG) SILICONE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410849886.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing silicone leathers are deficient in water resistance and stain resistance, resulting in short service life and easy contamination by microorganisms.

Method used

MQ silicone resin, modified organic montmorillonite-silica composite materials, flame retardants, catalysts and inhibitors are used to prepare waterproof silicone leather composite materials through processes such as kneading and planetary stirring, using new intercalation Agent (C/S)-q-PDMA was used for surface modification to enhance the hydrophobicity and stability of the composite material.

Benefits of technology

It achieves the excellent waterproofness, antifouling and durability of the composite material, improves the physical and chemical properties of the leather, and enhances its safety and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004916528330000111
    Figure BDA0004916528330000111
  • Figure BDA0004916528330000121
    Figure BDA0004916528330000121
Patent Text Reader

Abstract

The invention discloses a waterproof organic silicon leather composite material and a preparation method thereof. The organic silicon leather composite material is prepared from the following raw material components in parts by weight: 80 to 100 parts of MQ silicon resin, 25 to 50 parts of filler, 5 to 10 parts of hydrogen-containing silicone oil, 2 to 5 parts of flame retardant, 0.1 to 0.5 part of catalyst and 0.5 to 1 part of inhibitor. The waterproof organic silicon leather composite material is prepared by mixing the raw material components. Compared with the prior art, the modified organic montmorillonite-silicon dioxide composite material with the super-hydrophobic performance is prepared and used as a filler to be combined with the silicon resin and other raw materials in a reasonable proportion, so that the prepared organic silicon leather composite material has excellent waterproof performance and anti-pollution performance; and the stability and the durability are also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leather preparation, and in particular to a waterproof organic silicon leather composite material and a preparation method thereof. Background Art

[0002] Artificial leather is a plastic product that looks and feels like leather and is widely used in various fields. However, traditional artificial leather, such as polyurethane leather (PU), has many disadvantages. First, polyurethane itself is toxic and releases a large amount of harmful volatiles during the production process, posing a potential threat to the environment and human health. Second, the temperature resistance, aging resistance and breathability of traditional artificial leather are relatively poor, and the service life is short, making it difficult to meet the growing quality requirements.

[0003] Compared with traditional artificial leather, silicone leather, as a new type of leather material, has significant advantages. It adopts an environmentally friendly production process and does not release VOCs, which is fully in line with the concept of green development. In addition, silicone leather also has excellent stain resistance, weather resistance, high and low temperature resistance, and flame retardancy, allowing it to maintain stable performance in various environments. More importantly, the texture and appearance of silicone leather are similar to genuine leather, but the price is more affordable, providing consumers with more choices.

[0004] CN109056357A discloses a wear-resistant organic silicon leather and a preparation method thereof, which comprises the following components by mass fraction: 40-80 parts of base glue, 20-45 parts of phenyl silicone resin, 2-19 parts of Si-H-containing crosslinking agent, 0.01-1 parts of platinum catalyst, 0.0001-0.05 parts of inhibitor, 10-40 parts of filler, 0-10 parts of color paste, 0-10 parts of auxiliary agent, and 0-35 parts of organic solvent. Although the organic silicon leather provided by the invention has excellent wear resistance, it has poor water resistance, which not only limits the scope of use but also affects its service life.

[0005] CN115287911B discloses a waterproof and breathable organic silicon leather and a preparation method thereof, wherein the organic silicon leather comprises a leather base cloth, a microporous bottom layer and a microporous surface layer which are bonded and fixed in sequence from the inside to the outside, and a plurality of micro channels for ventilation are formed in the microporous bottom layer and the microporous surface layer, and the pore size of the micro channels is 0.2-5 μm. The leather has good waterproofness, breathability and weather resistance, and there is no release of molten droplets and toxic gases during the combustion process of the leather, and the leather has good environmental protection. Although the leather provided by the invention has excellent waterproof and breathable functions, its antifouling property is poor and it is easily contaminated by microorganisms, thereby causing damage to the leather. Summary of the invention

[0006] In view of the above-mentioned defects of the prior art, the present invention provides a waterproof organic silicone leather composite material, which not only has good stability and waterproofness, but also has excellent anti-fouling performance, is not easily contaminated by microorganisms, and increases its durability.

[0007] One of the purposes of the present invention is to provide a waterproof organic silicon leather composite material, which comprises the following raw material components in parts by weight:

[0008] MQ silicone resin 80-100 parts, filler 25-50 parts, hydrogen-containing silicone oil 5-10 parts, flame retardant 2-5 parts, catalyst 0.1-0.5 parts, inhibitor 0.5-1 parts.

[0009] Preferably, the MQ silicone resin is one or a mixture of two or more of methyl MQ silicone resin, methyl vinyl MQ silicone resin and methyl hydrogenated MQ silicone resin.

[0010] Preferably, the filler is a modified organic montmorillonite-silicon dioxide composite material, and its preparation method comprises the following steps, calculated by weight:

[0011] Dispersing 0.5-2 parts of montmorillonite, 0.4-0.6 parts of nano-silicon dioxide, and 2-4 parts of a modifier in 110-130 parts of anhydrous ethanol to obtain a suspension, then heating the suspension at 70-80° C. for 2.5-4.5 hours, then washing with anhydrous ethanol, collecting solid particles by centrifugation, and drying to obtain a modified organic montmorillonite-silicon dioxide composite material;

[0012] Or, 4-5 parts of montmorillonite are dispersed in 130-150 parts of water, heated to 75-85°C, and the pH is adjusted to 11.9-12.1 with a 0.1-0.3 mol / L sodium hydroxide aqueous solution to obtain a montmorillonite dispersion; 0.2-1 parts of an intercalating agent are dissolved in 45-60 parts of water, then added to the montmorillonite dispersion, stirred for 2.5-3.5 hours, then washed with water and centrifuged, solid particles are collected by centrifugation, and dried to obtain modified montmorillonite; 0.5-2 parts of modified montmorillonite, 0.4-0.6 parts of nano-silicon dioxide, and 2-4 parts of a modifier are dispersed in 110-130 parts of anhydrous ethanol to obtain a suspension, and then the suspension is heated at 70-80°C for 2.5-4.5 hours, then washed with anhydrous ethanol, solid particles are collected by centrifugation, and dried to obtain a modified organic montmorillonite-silicon dioxide composite material.

[0013] Preferably, the modifier is selected from at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, and 1H,1H,2H,2H-perfluorodecyltrimethoxysilane.

[0014] Preferably, the intercalant is (catechol / zwitterion) quaternized poly(dimethylamino)ethyl methacrylate, and its preparation method comprises the following steps, calculated by weight:

[0015] S1. Dissolve 0.7-1 parts of dimethylaminoethyl methacrylate and 0.8-1.2 parts of 2-chloro-3',4'-dihydroxyacetophenone in 45-55 parts of anhydrous ethanol, then add 4.8-5.2 parts of 0.035-0.45 g / mL ammonium persulfate aqueous solution and stir for 25-35 minutes to obtain a mixed solution A; then stir the mixed solution A at 65-75° C. for 46-55 hours, evaporate the solvent with a rotary evaporator, precipitate with cold ether, and dry the obtained precipitate under vacuum to obtain catechol quaternized poly(dimethylamino)ethyl methacrylate, referred to as Cq-PDMA;

[0016] S2. Dissolve 4.5-5.5 parts of Cq-PDMA and 6-6.2 parts of 1,3-propane sultone in a co-solvent prepared by mixing 90-110 parts of tetrahydrofuran and anhydrous ethanol in equal volumes, and then stir at 33-36° C. in a nitrogen atmosphere for 10-15 hours to obtain a mixed solution B; then evaporate the solvent from the mixed solution B in a rotary evaporator, and precipitate with cold ether. The obtained precipitate is dried under vacuum to obtain (catechol / zwitterion) quaternized polymethacrylate (dimethylamino)ethyl ester, referred to as (C / S)-q-PDMA.

[0017] Preferably, the flame retardant is selected from at least one of aluminum hydroxide, magnesium hydroxide and zinc borate.

[0018] Preferably, the catalyst is at least one of platinum black, chloroplatinic acid, platinum tetrachloride, chloroplatinic acid, and platinum tetrachloride.

[0019] Preferably, the inhibitor is selected from at least one of polyvinyl polysiloxane, amine compounds, phosphates, diallyl maleate, diethyl fumarate, methyl butynol, ethynyl cyclohexanol, phenyl butynol, and propyl butynol.

[0020] Preferably, the hydrogen-containing silicone oil is hydrogen-terminated poly(dimethylsiloxane). The second object of the present invention is to provide a method for preparing the waterproof organic silicone leather composite material, comprising the following steps:

[0021] Put MQ silicone resin and modified organic montmorillonite-silicon dioxide composite material into a kneading machine, knead for 40-50 minutes, then put into a planetary mixer, add flame retardant, hydrogen-containing silicone oil, catalyst, inhibitor, vacuum and stir and mix for 35-45 minutes to obtain a composite material for waterproof silicone leather.

[0022] Beneficial effects of the present invention:

[0023] 1. Compared with the prior art, the waterproof organic silicone leather composite material of the present invention has excellent waterproof and anti-fouling properties, good adhesion and is not easy to crack. The present invention adopts methyl vinyl MQ silicone resin as a substrate, and uses it in coordination with fillers, hydrogen-containing silicone oil, flame retardants, catalysts, and inhibitors in a reasonable proportion to prepare a waterproof organic silicone leather composite material, so that the composite material has good weather resistance, stain resistance, wear resistance and other properties, and at the same time forms good waterproof performance and anti-microbial contamination performance. The use of the waterproof organic silicone leather composite material provided by the present invention to prepare organic silicone leather not only improves the physical and chemical properties of organic silicone leather, but also enhances its safety and durability, bringing new development opportunities to the leather industry.

[0024] 2. The novel organic molecular intercalation agent (C / S)-q-PDMA prepared by the present invention is introduced into the interlayer of montmorillonite through ion exchange reaction to obtain intercalation modified montmorillonite, and then fluoroalkyl silane is introduced to perform surface modification on the intercalation modified montmorillonite and silica particles to prepare a montmorillonite-silicon dioxide composite material. Since the molecular size of (C / S)-q-PDMA molecules is larger than the original interlayer cations of montmorillonite, the insertion increases the interlayer distance of montmorillonite, provides space for surface modification, reduces uneven modification, and enhances the hydrophobicity of the composite material. Moreover, the (C / S)-q-PDMA molecule contains cationic (quaternary ammonium salt) and anionic (sulfonic acid) functional groups, and has zwitterionic properties. It can undergo ion exchange reactions with the surface of montmorillonite and silica particles to form zwitterionic structures, which enhance the binding force between them and improve the stability of the composite material. At the same time, it may provide additional electrostatic repulsion through zwitterions, hindering the close contact between cells and the leather surface, thereby reducing cell adhesion and the possibility of microbial contamination. In addition, the quaternary ammonium salt part of (C / S)-q-PDMA has a lower surface energy, which helps to reduce the van der Waals force and electrostatic force between particles, reduce aggregation, and improve the dispersibility of montmorillonite, thereby further improving the stability and durability of the composite material. DETAILED DESCRIPTION

[0025] Parameters for specific chemical substances used, sources.

[0026] Methyl vinyl MQ silicone resin, industrial grade, manufactured by Hubei Zhuoxuanyang International Trade Co., Ltd., item number: SH-5201 / 2;

[0027] Montmorillonite, particle size: 0.1-1 μm, Wuhan Kanos Technology Co., Ltd.;

[0028] Nano silicon dioxide, particle size 50-100nm, purity: 99.999%, produced by Zhejiang Manli Nano Technology Co., Ltd., item number: ML-SiO2;

[0029] Hydrogen-terminated poly(dimethylsiloxane), purity: 99%, manufacturer: Hubei Jusheng Technology Co., Ltd., item number: JS2110;

[0030] Methylbutynol, produced by Wuhan Jiyesheng Chemical Co., Ltd., CAS number: 115-19-5.

[0031] Example 1

[0032] A method for preparing a waterproof organic silicon leather composite material comprises the following steps:

[0033] 95 kg of methyl vinyl MQ silicone resin and 40 kg of modified organic montmorillonite-silica composite material were put into a kneading machine and kneaded for 45 minutes. Then, they were put into a planetary mixer, and 3 kg of zinc borate, 8 kg of hydrogen-terminated poly (dimethylsiloxane), 0.2 kg of platinum tetrachloride, and 0.8 kg of methyl butynol were added. The mixture was stirred and mixed in a vacuum for 40 minutes to obtain a composite material for silicone leather.

[0034] The preparation method of the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0035] 1.5 g of montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, which was then heated at 75° C. for 3 h, washed with anhydrous ethanol, and solid particles were collected by centrifugation and dried to obtain a modified organic montmorillonite-silica composite material.

[0036] Example 2

[0037] A method for preparing a waterproof organic silicon leather composite material, which is different from Example 1 in that the method for preparing the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0038] 1.5 g of montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, which was then heated at 75° C. for 3 h, washed with anhydrous ethanol, and solid particles were collected by centrifugation and dried to obtain a modified organic montmorillonite-silica composite material.

[0039] Example 3

[0040] A method for preparing a waterproof organic silicon leather composite material, which is different from Example 1 in that the method for preparing the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0041] 1.5 g of montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, which was then heated at 75° C. for 3 h, washed with anhydrous ethanol, and solid particles were collected by centrifugation and dried to obtain a modified organic montmorillonite-silica composite material.

[0042] Example 4

[0043] A method for preparing a waterproof organic silicon leather composite material comprises the following steps:

[0044] 95 kg of methyl vinyl MQ silicone resin and 40 kg of modified organic montmorillonite-silica composite material were put into a kneading machine and kneaded for 45 minutes. Then, they were put into a planetary mixer, and 3 kg of zinc borate, 8 kg of hydrogen-terminated poly (dimethylsiloxane), 0.2 kg of platinum tetrachloride, and 0.8 kg of methyl butynol were added. The mixture was stirred and mixed in a vacuum for 40 minutes to obtain a composite material for silicone leather.

[0045] The preparation method of the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0046] 4.5 g of montmorillonite was dispersed in 140 mL of water, heated to 80° C., and the pH was adjusted to 12 with a 0.2 mol / L sodium hydroxide aqueous solution to obtain a montmorillonite dispersion; 0.5 g of (C / S)-q-PDMA was dissolved in 50 mL of water, then added to the montmorillonite dispersion, stirred for 3 h, washed with water and centrifuged, solid particles were collected by centrifugation, and dried to obtain modified montmorillonite; 1.5 g of modified montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, and then the suspension was heated at 75° C. for 3 h, washed with anhydrous ethanol, solid particles were collected by centrifugation, and dried to obtain a modified organic montmorillonite-silica composite material.

[0047] The preparation method of the (C / S)-q-PDMA comprises the following steps:

[0048] S1. Dissolve 0.8 g of dimethylaminoethyl methacrylate and 1 g of 2-chloro-3',4'-dihydroxyacetophenone in 50 g of anhydrous ethanol, then add 5 g of 0.04 g / mL ammonium persulfate aqueous solution and stir for 30 min to obtain a mixed solution A; then stir the mixed solution A at 70° C. for 48 h, evaporate the solvent with a rotary evaporator, precipitate with cold ether, and dry the obtained precipitate under vacuum to obtain Cq-PDMA;

[0049] S2. Dissolve 5 g of Cq-PDMA and 6.1 g of 1,3-propane sultone in 100 mL of a co-solvent prepared by mixing tetrahydrofuran and anhydrous ethanol in equal volumes, and then stir at 35° C. under a nitrogen atmosphere for 12 h to obtain a mixed solution B; then evaporate the solvent of the mixed solution B in a rotary evaporator, and precipitate with cold ether. The resulting precipitate is dried under vacuum to obtain (C / S)-q-PDMA.

[0050] Example 5

[0051] A method for preparing a waterproof organic silicon leather composite material, which is different from Example 4 in that the method for preparing the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0052] 4.5 g of montmorillonite was dispersed in 140 mL of water, heated to 80° C., and the pH was adjusted to 12 with a 0.2 mol / L sodium hydroxide aqueous solution to obtain a montmorillonite dispersion; 0.2 g of (C / S)-q-PDMA was dissolved in 50 mL of water, then added to the montmorillonite dispersion, stirred for 3 h, washed with water and centrifuged, solid particles were collected by centrifugation, and dried to obtain modified montmorillonite; 1.5 g of modified montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, and then the suspension was heated at 75° C. for 3 h, washed with anhydrous ethanol, solid particles were collected by centrifugation, and dried to obtain a modified organic montmorillonite-silica composite material.

[0053] The preparation method of the (C / S)-q-PDMA is consistent with that of Example 4.

[0054] Example 6

[0055] A method for preparing a waterproof organic silicon leather composite material, which is different from Example 4 in that the method for preparing the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0056] 4.5 g of montmorillonite was dispersed in 140 mL of water, heated to 80° C., and the pH was adjusted to 12 with a 0.2 mol / L sodium hydroxide aqueous solution to obtain a montmorillonite dispersion; 1 g of (C / S)-q-PDMA was dissolved in 50 mL of water, then added to the montmorillonite dispersion, stirred for 3 h, washed with water and centrifuged, solid particles were collected by centrifugation, and dried to obtain modified montmorillonite; 1.5 g of modified montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, and then the suspension was heated at 75° C. for 3 h, washed with anhydrous ethanol, solid particles were collected by centrifugation, and dried to obtain a modified organic montmorillonite-silica composite material.

[0057] The preparation method of the (C / S)-q-PDMA is consistent with that of Example 4.

[0058] Comparative Example 1

[0059] A method for preparing a waterproof organic silicon leather composite material, which is different from Example 4 in that the method for preparing the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0060] 4.5 g of montmorillonite was dispersed in 140 mL of water, heated to 80° C., and the pH was adjusted to 12 with a 0.2 mol / L sodium hydroxide aqueous solution to obtain a montmorillonite dispersion; 0.5 g of hexadecyltrimethylammonium bromide was dissolved in 50 mL of water, then added to the montmorillonite dispersion, stirred for 3 h, washed with water and centrifuged, solid particles were collected by centrifugation, and dried to obtain modified montmorillonite; 1.5 g of modified montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, and then the suspension was heated at 75° C. for 3 h, washed with anhydrous ethanol, solid particles were collected by centrifugation, and dried to obtain a modified organic montmorillonite-silica composite material.

[0061] Comparative Example 2

[0062] A method for preparing a waterproof organic silicon leather composite material, which is different from Example 4 in that the method for preparing the modified organic montmorillonite-silicon dioxide composite material comprises the following steps:

[0063] 4.5 g of montmorillonite was dispersed in 140 mL of water, heated to 80° C., and the pH was adjusted to 12 with a 0.2 mol / L sodium hydroxide aqueous solution to obtain a montmorillonite dispersion; 0.5 g of octadecyltrimethylammonium bromide was dissolved in 50 mL of water, then added to the montmorillonite dispersion, stirred for 3 h, washed with water and centrifuged, solid particles were collected by centrifugation, and dried to obtain modified montmorillonite; 1.5 g of modified montmorillonite, 0.5 g of nano-silica, and 3 g of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, and then the suspension was heated at 75° C. for 3 h, washed with anhydrous ethanol, solid particles were collected by centrifugation, and dried to obtain a modified organic montmorillonite-silica composite material.

[0064] Comparative Example 3

[0065] A method for preparing a waterproof organic silicon leather composite material comprises the following steps:

[0066] 95 kg of methyl vinyl MQ silicone resin and 40 kg of modified organic montmorillonite were put into a kneading machine and kneaded for 45 minutes. Then, they were put into a planetary mixer, and 3 kg of zinc borate, 8 kg of hydrogen-terminated poly (dimethylsiloxane), 0.2 kg of platinum tetrachloride, and 0.8 kg of methyl butynol were added. The mixture was stirred and mixed in a vacuum for 40 minutes to obtain a composite material for silicone leather.

[0067] The preparation method of the modified organic montmorillonite material comprises the following steps:

[0068] 1.5 g of montmorillonite and 3 g of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane were dispersed in 120 mL of anhydrous ethanol to obtain a suspension, which was then heated at 75° C. for 3 h, washed with anhydrous ethanol, and solid particles were collected by centrifugation and dried to obtain a modified organic montmorillonite material.

[0069] Test Example 1

[0070] Leather performance test

[0071] Waterproof silicone leather preparation

[0072] The spunlace nonwoven fabric (Suzhou Aimee Medical Supplies Co., Ltd., width 10-330cm) was rinsed and dried to serve as a base fabric layer; the waterproof silicone leather composite material was coated on the base fabric layer to form a coating, and the coating was thinned to a thickness of 300 μm by an extrusion roller, and the coating was evenly adhered to the base fabric to form a leather body, and then cured; the cured leather body was subjected to a vacuum pattern suction machine to form different surface patterns, thereby obtaining waterproof silicone leather.

[0073] The waterproof silicone leather prepared by the above method for preparing the waterproof silicone leather was prepared using the waterproof silicone leather composite materials prepared in Examples 1-6 and Comparative Examples 1-3.

[0074] The leathers prepared in Examples 1-6, Comparative Examples 1-3, and commercially available leathers 1 and 2 were subjected to water drop angle tests, hot and cold shock tests, physical contamination resistance tests, and microbial contamination resistance tests, and the results are shown in Table 1.

[0075] Among them, the water drop angle test adopts the sessile drop method;

[0076] Thermal shock test: 60℃ / 25min, -20℃ / 25min, 150 cycles;

[0077] The reference test standard for the anti-physical pollution test is "GB / T 30159.1-2013 Testing and evaluation of anti-fouling properties of textiles";

[0078] Anti-microbial contamination test:

[0079] The growth characteristics of mouse fibroblast L929 are mainly wall-attached growth. This growth mode of close attachment to the surface can simulate the scene of microorganisms attaching to the leather surface, thus helping to more accurately evaluate the leather's anti-cell adhesion ability. Therefore, mouse fibroblast L929 was used to conduct silicone leather anti-microbial contamination test, and the percentage of cell adhesion can reflect the leather surface's adsorption capacity for cells, thereby indirectly indicating its anti-microbial contamination performance.

[0080] A high percentage of cell adhesion means that the leather surface has good cell affinity, and microorganisms are more likely to attach and grow on the leather surface, which indirectly reflects that it is susceptible to microbial contamination; on the contrary, a low percentage of cell adhesion indicates that microorganisms are not easy to attach and grow on the leather surface, and the leather is not easily contaminated by microorganisms.

[0081] (1) Cell culture: Mouse fibroblast L929 cells (Shanghai Meiyan Biotechnology Co., Ltd.) were cultured in RPMI 1640 medium containing 10% fetal bovine serum (FBS), 1% (100 μg / mL) penicillin and 1% (100 μg / mL) streptomycin.

[0082] (2) Cell adhesion assay: Before the experiment, the surface of the sample to be tested was disinfected, and the sample was placed in a 48-well plate and irradiated with ultraviolet light for 40 min in a sterile operating table before use. 1×10 4 cells, incubated in the incubator for 24 hours and then removed. After the culture medium in the well was aspirated, 4% paraformaldehyde solution was added to fix for 10 minutes, washed three times with sterile phosphate buffer (PH = 7.4), and then the membrane was broken with 0.1% TritonX-100 solution for 5 minutes, and washed three times with phosphate buffer (PH = 7.4). 4',6-diamidino-2-phenylindole (DAPI) staining: Add an appropriate amount of DAPI staining solution diluted in a certain proportion and spread it on the sample surface, absorb the dye after 10 minutes, and wash it three times with phosphate buffer (PH = 7.4). The antifouling behavior was studied using optical microscopy and scanning electron microscopy (SEM). The experiment was repeated three times, and three sets of parallel samples were kept each time.

[0083] Table 1 Performance test of silicone leather

[0084]

[0085]

[0086] From the test results in Table 1, it can be seen that the water drop angle of the organic silicon leather described in Examples 1-6 and Comparative Examples 1-2 exceeds 100°, and has a surface hydrophobic effect. Among them, the water drop angle of Examples 4-5 is greater than that of Examples 1-3 and Comparative Examples 1-2, exceeding 125°, and has excellent hydrophobic properties. The reason for the analysis may be that the modified organic montmorillonite-silicon dioxide composite material with super hydrophobic properties is introduced as a filler and used in combination with silicone resin, so that the prepared organic silicon leather has excellent waterproof properties. Nano-silicon dioxide can fill the voids of montmorillonite. Therefore, the combination of the microstructure of montmorillonite and the nanostructure of silicon dioxide can form an almost continuous rough surface, giving the montmorillonite-silicon dioxide composite material a high surface roughness, resulting in it having high hydrophobic properties. On this basis, in order to improve the hydrophobicity and stability of the composite material, the present invention introduces (C / S)-q-PDMA into the interlayer of montmorillonite through an ion exchange reaction. The (C / S)-q-PDMA molecule contains a cation (quaternary ammonium salt) and an anion (sulfonic acid group) functional group to form a zwitterionic structure, so that it can interact with the charge sites on the surface of the silica particles, thereby enhancing the binding force between montmorillonite and silica and improving the stability of the composite material. In order to further improve the hydrophobicity of the composite material, the present invention also introduces 1H, 1H, 2H, 2H-perfluorodecyl trimethoxysilane to modify the surface of montmorillonite and silica particles, reducing the surface energy of the material surface, generating hydrophobic particles, and because the molecular size of (C / S)-q-PDMA is larger than the size of the original interlayer cation of montmorillonite, the insertion of the (C / S)-q-PDMA molecule leads to an increase in the interlayer distance of montmorillonite, providing space for surface modification, reducing the situation of uneven modification, thereby further improving the hydrophobicity of the composite material.

[0087] It can be seen from the hot and cold shock test results of Table 1 that embodiments 4-6 and comparative examples 1-2 have excellent stability under significant temperature changes, while embodiments 1-3 and comparative examples 3 and commercially available 1-2 leathers have poor stability. The reason for the analysis may be that 1H, 1H, 2H, 2H-perfluorodecyl trimethoxysilane modification introduces low surface energy fluorocarbon segments on the surface of montmorillonite and silica particles, causing the particle surface to become hydrophobic, and particles may aggregate due to hydrophobic interactions, thereby affecting material dispersibility. Charged organic molecules (C / S)-q-PDMA are introduced into the montmorillonite interlayer by ion exchange reaction, resulting in an increase in the interlayer spacing of montmorillonite, which helps to increase the degree of freedom between montmorillonite layers, thereby promoting its dispersibility to increase. In addition, the quaternary ammonium salt on (C / S)-q-PDMA has a lower surface energy, which helps to reduce the van der Waals force and electrostatic force between montmorillonite particles, reduces the aggregation phenomenon of particles, thereby improving its dispersibility. The improved dispersion of the organic montmorillonite-silica composite material helps to disperse the thermal stress more evenly under hot and cold shocks, reducing the risk of cracks and deformation on the leather surface, thereby improving the toughness and service life of the leather.

[0088] From the anti-physical pollution test results in Table 1, it can be seen that the anti-fouling performance of the silicone leather of Examples 1-6 and Comparative Examples 1-2 all reached level 4 or above, indicating that they have good resistance to liquid dirt and solid dirt. At the same time, Comparative Example 3 and Commercially Available 1-2 are both below level 3, and the anti-fouling performance is poor. The reason for this may be that the super-hydrophobic surface of the silicone leather can reduce the adhesion of water and other liquids, so that water droplets can take away dust and dirt on the surface, thereby keeping the surface clean, and thus having excellent anti-fouling performance.

[0089] It can be seen from the antimicrobial contamination test results of Table 1 that the cell adhesion percentages of Examples 1-3, Comparative Examples 1-3 and Commercially Available 1-2 are all higher than 90%, while the cell adhesion percentages of Examples 4-6 are lower than 6%, with excellent anti-cell adhesion properties, indicating that they are less likely to be contaminated by microorganisms. The reason for the analysis may be that (C / S)-q-PDMA is introduced into the interlayer of montmorillonite by ion exchange reaction, and (C / S)-q-PDMA has both cationic (quaternary ammonium salt) and anionic (sulfonic acid) functional groups, which may hinder the close contact between cells and leather surfaces by providing additional electrostatic repulsion, thereby reducing cell adhesion. 1H, 1H, 2H, 2H-perfluorodecyl trimethoxysilane was then used to surface modify montmorillonite and silica particles to prepare an organic montmorillonite-silica composite material with super hydrophobicity. The introduction of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane makes the coating surface have a lower surface energy, resulting in a weakened interaction with biological molecules, thereby reducing the possibility of cell adhesion. At the same time, the addition of silica increases the surface roughness and forms a micro-nanoscale rough structure. This rough structure helps to capture air and further enhance the hydrophobicity and anti-cell adhesion properties of the coating.

Claims

1. A waterproof organic silicon leather composite material, characterized in that: By weight, it includes the following raw material components: MQ silicone resin 80-100 parts, filler 25-50 parts, hydrogen-containing silicone oil 5-10 parts, flame retardant 2-5 parts, catalyst 0.1-0.5 parts, inhibitor 0.5-1 parts.

2. The waterproof organic silicon leather composite material according to claim 1, characterized in that: The MQ silicone resin is one or a mixture of two or more of methyl MQ silicone resin, methyl vinyl MQ silicone resin and methyl hydrogenated MQ silicone resin.

3. The waterproof organic silicon leather composite material according to claim 1, characterized in that: The filler is a modified organic montmorillonite-silicon dioxide composite material, and its preparation method comprises the following steps, calculated by weight: Dispersing 0.5-2 parts of montmorillonite, 0.4-0.6 parts of nano-silicon dioxide, and 2-4 parts of a modifier in 110-130 parts of anhydrous ethanol to obtain a suspension, then heating the suspension at 70-80° C. for 2.5-4.5 hours, then washing with anhydrous ethanol, collecting solid particles by centrifugation, and drying to obtain a modified organic montmorillonite-silicon dioxide composite material; Alternatively, 4-5 parts of montmorillonite are dispersed in 130-150 parts of water, heated to 75-85° C., and the pH is adjusted to 11.9-12.1 with a 0.1-0.3 mol / L sodium hydroxide aqueous solution to obtain a montmorillonite dispersion; 0.2-1 parts of an intercalating agent are dissolved in 45-60 parts of water, and then added to the montmorillonite dispersion, stirred for 2.5-3.5 hours, then washed with water and centrifuged, solid particles are collected by centrifugation, and dried to obtain modified montmorillonite; 0.5-2 parts of modified montmorillonite, 0.4-0.6 parts of nano-silicon dioxide, and 2-4 parts of a modifier are dispersed in 110-130 parts of anhydrous ethanol to obtain a suspension, and then the suspension is heated at 70-80°C for 2.5-4.5 hours, then washed with anhydrous ethanol, solid particles are collected by centrifugation, and dried to obtain a modified organic montmorillonite-silicon dioxide composite material.

4. The waterproof organic silicon leather composite material according to claim 3, characterized in that: The modifier is selected from at least one of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, and 1H,1H,2H,2H-perfluorodecyltrimethoxysilane.

5. The waterproof organic silicon leather composite material according to claim 3, characterized in that: The intercalant is (catechol / zwitterion) quaternized poly(dimethylamino)ethyl methacrylate, and its preparation method comprises the following steps, calculated by weight: S1. Dissolve 0.7-1 parts of dimethylaminoethyl methacrylate and 0.8-1.2 parts of 2-chloro-3',4'-dihydroxyacetophenone in 45-55 parts of anhydrous ethanol, then add 4.8-5.2 parts of 0.035-0.45 g / mL ammonium persulfate aqueous solution and stir for 25-35 minutes to obtain a mixed solution A; then stir the mixed solution A at 65-75° C. for 46-55 hours, evaporate the solvent with a rotary evaporator, precipitate with cold ether, and dry the obtained precipitate under vacuum to obtain catechol quaternized poly(dimethylamino)ethyl methacrylate, referred to as Cq-PDMA; S2. Dissolve 4.5-5.5 parts of Cq-PDMA and 6-6.2 parts of 1,3-propane sultone in a co-solvent prepared by mixing 90-110 parts of tetrahydrofuran and anhydrous ethanol in equal volumes, and then stir at 33-36° C. in a nitrogen atmosphere for 10-15 hours to obtain a mixed solution B; then evaporate the solvent from the mixed solution B in a rotary evaporator, and precipitate with cold ether. The obtained precipitate is dried under vacuum to obtain (catechol / zwitterion) quaternized polymethacrylate (dimethylamino)ethyl ester, referred to as (C / S)-q-PDMA.

6. The waterproof organic silicon leather composite material according to claim 1, characterized in that: The flame retardant is selected from at least one of aluminum hydroxide, magnesium hydroxide and zinc borate.

7. The waterproof organic silicon leather composite material according to claim 1, characterized in that: The catalyst is at least one of platinum black, chloroplatinic acid and platinum tetrachloride.

8. The waterproof organic silicon leather composite material according to claim 1, characterized in that: The inhibitor is selected from at least one of polyvinyl polysiloxane, amine compounds, phosphates, diallyl maleate, diethyl fumarate, methyl butynol, ethynyl cyclohexanol, phenyl butynol, and propyl butynol.

9. The waterproof organic silicon leather composite material according to claim 1, characterized in that: The hydrogen-containing silicone oil is hydrogen-terminated poly(dimethylsiloxane).

10. The method for preparing the waterproof organic silicon leather composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Put MQ silicone resin and modified organic montmorillonite-silicon dioxide composite material into a kneading machine, knead for 40-50 minutes, then put into a planetary mixer, add flame retardant, hydrogen-containing silicone oil, catalyst, inhibitor, vacuum and stir and mix for 35-45 minutes to obtain a composite material for waterproof silicone leather.