Super-hydrophobic coating as well as preparation method and application thereof

Through a combination of specific proportions of amino-terminated silicone fluororesin, modified epoxy resin and modified nano-silica, the problem of insufficient mechanical properties of traditional hydrophobic coatings is solved, and efficient super-hydrophobic coating preparation is achieved with good performance. Excellent adhesion and physical properties for building materials, electronics and automotive applications.

CN118755346APending Publication Date: 2024-10-11SHANGHAI COOVER NEW MATERIAL CO LTD

Patent Information

Application Number
CN202410869255.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Traditional hydrophobic coatings have problems in mechanical properties such as low hardness, poor wear resistance, weak adhesion and poor performance after aging, which limits their use in practical applications.

Method used

Using a specific ratio of amino-terminated silicone fluorine resin, modified epoxy resin and modified nano-silica, by adjusting the mass ratio of aminosilicone and fluorosilicone, and the molar ratio of epoxy resin and long carbon chain fatty acid The ratio, the particle size of the nano-silica and the surface treatment agent are combined to form a coating with super hydrophobicity and good physical properties.

Benefits of technology

It achieves excellent hydrophobicity of the coating, improves adhesion and mechanical properties, and reduces costs, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004921143860000051
    Figure BDA0004921143860000051
  • Figure BDA0004921143860000052
    Figure BDA0004921143860000052
  • Figure BDA0004921143860000061
    Figure BDA0004921143860000061
Patent Text Reader

Abstract

The invention relates to the technical field of hydrophobic coatings, in particular to IPC C09D163 / 00, and more particularly relates to a super-hydrophobic coating and a preparation method and application thereof.The super-hydrophobic coating is prepared from, by mass, 18-48 parts of A component amino-terminated silicon-fluorine resin, 45-75 parts of B component modified epoxy resin and 4-9 parts of C component modified nano silicon dioxide; the amino-terminated silicon-fluorine resin is prepared from the following raw materials: amino siloxane and fluorine-containing siloxane. Modified epoxy resin is adopted as a coating main body, amino-terminated silicon-fluorine resin which has super-hydrophobicity and can react with the modified epoxy resin is innovatively synthesized to serve as a coating frame, and a microcosmic uneven structure is formed under the comprehensive action of modified nano silicon dioxide. Therefore, the surface of the coating has a lotus-leaf-surface-shaped super-hydrophobic structure, and the coating has excellent hydrophobicity and good physical properties under the compounding action of the three layers of materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrophobic coatings, in particular to IPC C09D163 / 00, and more specifically to a super hydrophobic coating and a preparation method and application thereof. Background Art

[0002] Super-hydrophobic coating with high water drop angle (>150 °) has broad application prospects in liquid anti-sticking and self-cleaning, etc. So far, people have reported many super-hydrophobic coating materials, and prior art CN101575478A discloses a preparation method of epoxy resin super-hydrophobic coating, and the method dissolves silicon dioxide particles in a solvent, adds silane coupling agent, epoxy resin, hydrophobic agent to obtain coating sol, and then evenly applies to substrate surface, and finally heats to make epoxy resin curing crosslinking, i.e., obtain epoxy resin super-hydrophobic coating. However, traditional hydrophobic coating is usually limited in mechanical properties, such as its low hardness, poor wear resistance, weak adhesion with substrate, poor performance after aging, and other problems seriously hinder the practical application of super-hydrophobic coating. Therefore, developing a coating method with super-hydrophobicity has important application value. Summary of the invention

[0003] In order to solve the problems in the prior art, the first aspect of the present invention provides a super hydrophobic coating, the raw materials for its preparation, by mass, include 18-48 parts of amino-terminated silicone fluororesin as component A, 45-75 parts of modified epoxy resin as component B, and 4-9 parts of modified nano-silica as component C. The raw materials for the preparation of the amino-terminated silicone fluororesin include aminosiloxane and fluorine-containing silicone.

[0004] Preferably, the mass ratio of the aminosilicone to the fluorine-containing silicone is 100:30-100.

[0005] Furthermore, the mass ratio of the aminosilicone to the fluorine-containing silicone is 100:60-100.

[0006] The applicant's creative research found that when the aminosilicone mass ratio exceeds the range, the fluorine content of the system will be reduced, resulting in a decrease in the hydrophobicity of the coating. At the same time, the curing speed is too fast, which makes the shrinkage pressure of the coating too large during curing, which will reduce the adhesion of the coating; when the aminosilicone ratio is too low, it will lead to incomplete curing of the coating, resulting in a decrease in the mechanical properties of the coating. In particular, when the mass ratio of aminosilicone to fluorine-containing silicone is 100:30-100, the performance is particularly outstanding.

[0007] Preferably, the aminosiloxane includes one or more of 3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane, anilinomethyltrimethoxysilane, and aminoethylaminopropyltrimethoxysilane.

[0008] Preferably, the fluorine-containing silicone includes one or more of heptadecafluorodecylsiloxane, (nonafluorohexyl)siloxane, and methyl(trifluoropropyl)siloxane.

[0009] Preferably, the raw materials for preparing the amino-terminated silicone fluororesin further include 1% pure water and 1% ethanol.

[0010] Preferably, the mass ratio of the total mass of the aminosilicone and the fluorinated silicone to the ethanol 1 is 0.3-1:1.

[0011] Preferably, the mass ratio of the pure water 1 to the ethanol 1 is 0.1-0.2:1.

[0012] Preferably, the preparation method of the amino-terminated silicone fluororesin comprises the following steps:

[0013] S1: aminosilicone, fluorinated silicone, and ethanol 1 are placed in a reaction kettle and stirred, and pure water 1 is added after adjusting the pH value to 3.0-3.5 to obtain a mixed solution;

[0014] S2: heating the mixed solution in the reactor to 70-80°C and stirring the mixture for 8-10 hours until the mixed solution becomes milky, and then vacuuming the mixture to obtain the reaction product;

[0015] S3: Dry the reaction product in S2 for 2-3 hours to obtain component A.

[0016] Furthermore, acetic acid is used to adjust the pH value in S1.

[0017] Preferably, the raw materials for preparing the modified epoxy resin include epoxy resin and long-chain fatty acid; the molar ratio of the epoxy group of the epoxy resin to the carboxyl group of the long-chain fatty acid is 1:0.2-0.5.

[0018] When the carboxyl group ratio is too high, too many long-chain hydrophobic groups will be introduced into the molecular chain of the finished product, which will reduce the bonding strength between the cured epoxy coating and the substrate, resulting in poor mechanical properties of the overall coating and loss of practical use value; when the carboxyl group ratio is too low, too few long-chain hydrophobic groups will be introduced into the molecular chain of the finished product, thereby reducing the hydrophobic performance of the coating and failing to meet the ideal water drop angle requirements. The applicant has found through a large number of creative experiments that when the molar ratio of the epoxy group of the epoxy resin to the carboxyl group of the long carbon chain fatty acid is 1:0.2-0.5, the coating has excellent hydrophobicity and good physical properties.

[0019] Preferably, the epoxy resin includes one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, and alicyclic epoxy resin.

[0020] Preferably, the long carbon chain fatty acid includes one or more of sebacic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, and pentadecanedioic acid.

[0021] Preferably, the preparation method of the modified epoxy resin comprises the following steps:

[0022] S6: Add epoxy resin and long-chain fatty acid to the reactor, start stirring, heat the reaction to 120°C, maintain the temperature for 4-5 hours, take a small sample of 10 grams and drop it into 0°C ice water for observation. When uniform milk-like flocs appear, the reaction is over. Cool the reactor and start discharging when the temperature drops to 30°C to obtain product component B.

[0023] Furthermore, the condition for the end of the reaction in S6 is: take a small sample of 10 grams and drop it into 0°C ice water for observation. The reaction is ended when uniform milky flocs appear.

[0024] Preferably, the raw materials for preparing the modified nano-silica include nano-silica, a surface treatment agent, 2 ethanol, and 2 pure water.

[0025] Preferably, the particle size of the nano-silicon dioxide is less than 300 nm.

[0026] Preferably, the surface treatment agent includes one or more of 3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldiethoxysilane, phenylaminomethyltriethoxysilane, phenylaminomethyltrimethoxysilane, and aminoethylaminopropyltrimethoxysilane.

[0027] The applicant has found through a large number of creative experiments that the particle size of nano-silica is below 300nm. If silica with a particle size of micron level is used, the microstructure of the coating will lack nano-level tiny protrusions, and the coating structure cannot constitute a microstructure similar to the surface of a lotus leaf, thus there will be no super-hydrophobic effect; through the surface-coated silane coupling agent, the fine inorganic silica particles are chemically bonded to the epoxy organic resin system, which, on the one hand, greatly enhances the compatibility between inorganic and organic, and on the other hand, allows the silica to be dispersed in the system to act as an anchor point, reducing the sliding of the molecular chain, so that the coating exhibits better mechanical properties.

[0028] Preferably, the mass ratio of the nano-silicon dioxide to the pure water 2 is 1:2.

[0029] Preferably, the mass ratio of the ethanol 2 to the pure water 2 is 3:1.

[0030] Preferably, the mass ratio of the surface treatment agent to nano-silicon dioxide is 0.01-0.1:1.

[0031] Preferably, the preparation method of the modified nano-silicon dioxide comprises the following steps:

[0032] S7: Add nano-silicon dioxide and pure water 2 to the reactor and stir evenly. Then add ethanol 2 and slowly stir and disperse at room temperature for 30 minutes. After the dispersion is completed, add the surface treatment agent, heat to 60°C and keep stirring for 1 hour. Then vacuumize and dry at 120°C and grind to obtain component C.

[0033] In the present invention, ethanol 1 and ethanol 2 are the same substance, pure water 1 and pure water 2 are the same substance, and the above names are only used for distinction.

[0034] A second aspect of the present invention provides a method for preparing a super-hydrophobic coating, comprising the following steps:

[0035] S4: Add component B and component C into the material tank of the double planetary disperser and mix them evenly;

[0036] S5: Continue to add component A and stir evenly under vacuum to obtain the super hydrophobic coating.

[0037] Furthermore, in the step S5, the material temperature is controlled at 18-28°C during the stirring process.

[0038] A third aspect of the present invention provides the use of the above-mentioned super-hydrophobic coating in surface coating of materials in the fields of building materials, electronic products, and automobiles.

[0039] Beneficial Effects

[0040] 1. The super hydrophobic coating prepared by the present invention adopts a specific modified epoxy resin as the coating body. When the molar ratio of the epoxy group of the epoxy resin to the carboxyl group of the long carbon chain fatty acid is 1:0.2-0.5, the coating has good physical properties while ensuring excellent hydrophobicity.

[0041] 2. The super hydrophobic coating prepared by the present invention adopts a specially prepared amino-terminated fluorosilicone resin as the coating frame. When the mass ratio of aminosilicone to fluorosilicone is 100:30-100, the adhesion of the coating can be improved while ensuring that the coating has excellent hydrophobicity.

[0042] 3. The super hydrophobic coating prepared by the present invention adopts a specific modified nano-silica, which can improve the mechanical properties of the coating while ensuring that the coating has excellent hydrophobicity.

[0043] 4. The present invention adopts modified epoxy resin as the main body of the coating, and innovatively synthesizes an amino-terminated silicone-fluororesin that has both super-hydrophobicity and the ability to react with the modified epoxy resin as the coating framework, and the combined effect of modified nano-silicon dioxide forms a microscopic uneven structure, so that the coating surface has a super-hydrophobic structure like a lotus leaf surface. After the composite effect of the three layers of materials, the coating has excellent hydrophobicity and good physical properties.

[0044] 5. The raw materials of the super-hydrophobic coating of the present invention are easily available, easy to prepare, low in cost, and easy to industrially produce. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The experimental methods in the examples without specifying specific conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0046] The raw material types and their sources in the embodiments and comparative examples are as follows:

[0047] γ-Aminopropyltrimethoxysilane: Zhengzhou Aikemu Chemical Co., Ltd. CAS: 13822-56-5;

[0048] N-β(aminoethyl)-γ-aminopropylmethyldimethoxysilane: Hangzhou Jessica Chemical Co., Ltd. CAS: 3069-29-2;

[0049] Phenylaminomethyltrimethoxysilane: Nanjing Quanxi New Materials Co., Ltd. CAS: 77855-73-3;

[0050] Heptadecafluorodecylsiloxane: Guangzhou Ruishi Biotechnology Co., Ltd. CAS: 83048-65-1;

[0051] (Nonafluorohexyl)siloxane: Tianmen Hengchang Chemical Co., Ltd. CAS: 85877-79-8;

[0052] Glycidyl ether epoxy resin / DER383: Dow Chemical CAS: 25068-38-6;

[0053] Dodecacarbon long-chain dibasic acid: Zhonghe Chemical (Shandong) Co., Ltd. CAS: 693-23-2;

[0054] Nano-silicon dioxide: Foshan Oulite New Material Technology Co., Ltd. 200nm CAS: 14808-60-7;

[0055] γ-Aminopropyltriethoxysilane: Nanjing Xuanhao New Materials Co., Ltd. CAS: 919-30-2.

[0056] Examples 1-8, Comparative Examples 1-3

[0057] Embodiments 1-8 and comparative examples 1-3 of the present invention provide a super hydrophobic coating, and the formula is shown in Tables 1-4 in parts by mass: Table 1 is the composition and mass ratio of each substance of component A, Table 2 is the composition and molar ratio of each substance of component B, Table 3 is the composition and mass ratio of each substance of component C, and Table 4 is the composition and mass ratio of each substance of the super hydrophobic coating composition. The blanks in the following tables represent that this substance is not contained.

[0058] Table 1

[0059]

[0060] Table 2

[0061]

[0062] Table 3

[0063]

[0064] Table 4

[0065]

[0066] The preparation method of the amino-terminated silicone fluororesin described in Examples 1-8 and Comparative Examples 1-3 of the present invention comprises the following steps:

[0067] S1: aminosilicone, fluorinated silicone, and ethanol 1 are placed in a reaction kettle and stirred, and pure water 1 is added after adjusting the pH value to 3.1 with acetic acid to obtain a mixed solution;

[0068] S2: heating the mixed solution in the reactor to 72°C and stirring the mixture for 9 hours until the mixed solution becomes milky, and then vacuuming the mixture to obtain the reaction product;

[0069] S3: Dry the reaction product in S2 for 2 h to obtain component A.

[0070] The preparation method of the modified epoxy resin comprises the following steps:

[0071] S6: Add epoxy resin and long-chain fatty acid to the reactor, start stirring, heat the reaction to 120°C, maintain the temperature for 4.5 hours, and then the reaction is completed. Cool the reactor, and start discharging when the temperature drops to 35°C to obtain product component B.

[0072] The preparation method of the modified nano silicon dioxide comprises the following steps:

[0073] S7: Add nano-silicon dioxide and pure water 2 to the reactor and stir evenly. Then add ethanol 2 and slowly stir and disperse at room temperature for 30 minutes. After the dispersion is completed, add the surface treatment agent, heat to 60°C and keep stirring for 1 hour. Then vacuumize and dry at 120°C and grind to obtain component C.

[0074] The second aspect of the embodiments 1-8 and comparative examples 1-3 of the present invention provides a method for preparing a super-hydrophobic coating, comprising the following steps: S4: adding component B and component C into a material cylinder of a double planetary disperser and stirring evenly;

[0075] S5: Continue to add component A and stir evenly under vacuum. During the stirring process, the material temperature is controlled at 20° C. to obtain the super hydrophobic coating.

[0076] The third aspect of Examples 1-8 and Comparative Examples 1-3 of the present invention provides the application of the above-mentioned super-hydrophobic coating in the surface coating of materials in the fields of building materials, electronic products, and automobiles.

[0077] Performance Testing

[0078] Sample preparation:

[0079] Test substrate: aluminum sheet

[0080] Coating: The super hydrophobic coatings prepared in Examples 1-8 of the present invention and Comparative Examples 1-3 and commercially available products (UV curing solution, car cover film coating) are coated on the aluminum sheet by roller coating, shower coating or brush coating. The thickness is controlled to be about 10-20 microns.

[0081] Curing: Curing at room temperature 25℃ for 48h.

[0082] test:

[0083] 1. Water drop angle test: Instrument: Water drop angle tester, more than 150° is qualified.

[0084] 2. Hardness test: The instrument is a pencil hardness tester.

[0085] 3. Adhesion test: The test method is the hundred-grid method.

[0086] 4. Wear resistance test: Steel wool model 0000#, 500g pressure, reciprocating distance 40cm, 5000 times, and then do a water drop angle test, it is qualified if it is greater than or equal to 150°.

[0087] 5. Double 85 aging test: Place the sample in an aging box at 85°C and 85% humidity for 500 hours and then test the adhesion and water drop angle. If the adhesion does not decay, it is qualified. If the water drop angle is greater than 150°, it is qualified. The performance test results of each embodiment and comparative example are shown in Table 5.

[0088] Table 5

[0089]

Claims

1. A super hydrophobic coating, characterized in that: The raw materials for preparing the amino-terminated silicone fluorine resin include 18-48 parts of component A amino-terminated silicone fluorine resin, 45-75 parts of component B modified epoxy resin, and 4-9 parts of component C modified nano silicon dioxide. The raw materials for preparing the amino-terminated silicone fluorine resin include aminosilicone and fluorine-containing silicone.

2. The super-hydrophobic coating according to claim 1, characterized in that The mass ratio of the aminosilicone to the fluorine-containing silicone is 100:30-100.

3. The super-hydrophobic coating according to claim 2, characterized in that The aminosiloxane includes one or more of 3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldiethoxysilane, anilinomethyltriethoxysilane, anilinomethyltrimethoxysilane, and aminoethylaminopropyltrimethoxysilane.

4. The super-hydrophobic coating according to claim 2, characterized in that The fluorine-containing silicone includes one or more of heptadecafluorodecylsiloxane, (nonafluorohexyl)siloxane, and methyl (trifluoropropyl)siloxane.

5. The super hydrophobic coating according to claim 2, characterized in that The preparation method of the amino-terminated silicone fluororesin comprises the following steps: S1: aminosilicone, fluorinated silicone, and ethanol 1 are placed in a reaction kettle and stirred, and pure water 1 is added after adjusting the pH value to 3.0-3.5 to obtain a mixed solution; S2: heating the mixed solution in the reactor to 70-80°C and stirring the mixture for 8-10 hours until the mixed solution becomes milky, and then vacuuming the mixture to obtain the reaction product; S3: Dry the reaction product in S2 for 2-3 hours to obtain component A.

6. The super hydrophobic coating according to claim 1, characterized in that The raw materials for preparing the modified epoxy resin include epoxy resin and long-chain fatty acid; the molar ratio of the epoxy group of the epoxy resin to the carboxyl group of the long-chain fatty acid is 1:0.2-0.

5.

7. The super hydrophobic coating according to claim 6, characterized in that The epoxy resin includes one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, and alicyclic epoxy resin.

8. The super hydrophobic coating according to claim 6, characterized in that The long carbon chain fatty acid includes one or more of sebacic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, and pentadecanedioic acid.

9. A method for preparing a super-hydrophobic coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: S4: Add component B and component C into the material tank of the double planetary disperser and mix them evenly; S5: Continue to add component A and stir evenly under vacuum to obtain the super hydrophobic coating.

10. Application of the super-hydrophobic coating according to any one of claims 1 to 8 in surface coating of materials in the fields of building materials, electronic products and automobiles.

Citation Information

Patent Citations

  • Method for preparing epoxy resin super-hydrophobic coat

    CN101575478A

  • Water-based fluorine-containing epoxy paint

    CN103571302A

  • Super-hydrophobic paint composition and super-hydrophobic coating therewith

    CN104513585A

  • Amphiphobic layer and printing ink packaging film containing same

    CN107502165A

  • Preparation method and application of amino fluorosilicone resin and composition thereof

    CN111925525A

Cited By

  • Marine cable with built-in control cable in cable core

    CN121355017A