Water-based roller coating as well as preparation method and application thereof

By developing a water-based roller spray coating for NdFeB magnets, using a specific proportion of water-based epoxy resin and other additives, the problem of low coating efficiency and insufficient chemical resistance of small-sized NdFeB magnets has been solved. problem, achieving efficient, environmentally friendly coating film coverage and improved chemical resistance.

CN118755352AActive Publication Date: 2024-10-11HUNAN SOKAN NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411006370.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

It is difficult to effectively coat parts made of small-sized NdFeB magnets with existing technology. Conventional spraying methods are inefficient and waste resources. Moreover, conventional epoxy coatings have limited chemical resistance and can easily lead to adhesion problems.

Method used

Develop a water-based roller spray coating, using 30 to 45 parts of the first water-based epoxy resin, 10 to 15 parts of the second water-based epoxy resin, 1 to 2 parts of dispersant, 1 to 20 parts of water, 5 to 10 parts of filler, 0.1 ~0.5 parts of pH regulator and 3~5 parts of amino resin are used to achieve uniform coverage of the coating film through the roller spray process. It is combined with defoaming agents, wetting agents, film-forming aids and adhesion promoters to improve the construction of the coating. properties and chemical resistance.

Benefits of technology

It achieves a film thickness of 5 to 15 μm after a single roll coating, which significantly saves production time. It has excellent chemical resistance, can pass the 72-hour oleic acid immersion test under high temperature and high humidity conditions, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963116560000043
    Figure BDA0004963116560000043
  • Figure BDA0004963116560000051
    Figure BDA0004963116560000051
  • Figure BDA0004963116560000052
    Figure BDA0004963116560000052
Patent Text Reader

Abstract

The invention discloses a water-based roll spray coating as well as a preparation method and application thereof. The water-based roll spray coating is prepared from the following raw materials in parts by weight: 30-45 parts of first water-based epoxy resin, 10-15 parts of second water-based epoxy resin, 1-2 parts of a dispersing agent, 1-20 parts of water, 5-10 parts of filler, 0.1-0.5 part of a pH regulator and 3-5 parts of amino resin. A water-based system is adopted, so that the environment-friendly requirement is met; the paint has excellent chemical resistance, and is free of abnormity after being soaked in oleic acid for 72 hours at high temperature and high humidity; the required film thickness is low, the film is suitable for being applied to a small-size neodymium iron boron magnetic steel material, and the performance test in a table can be met when the minimum film thickness is 5 microns; the coating has good constructability, materials with the maximum thickness of 40 microns or above are not adhered to one another after being sprayed for one time, and the production time is greatly saved compared with the mode that the target film thickness is achieved through multiple times of rolling spraying.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a water-based rolling spray coating and a preparation method and application thereof. Background Art

[0002] At present, small-sized NdFeB magnet parts are increasingly widely used in the market, but because they are mostly special-shaped parts with small sizes, conventional spraying methods such as automatic line spraying cannot achieve good coating. Therefore, people have developed a variety of spraying methods for this material. There are two common ones: one is to use conventional epoxy paint, spray one side with a reciprocating machine, and then turn it over and spray the other side after curing. This method is very inefficient; the other is the roller spraying process, which puts the material and the accompanying plating material into the roller spraying machine together, and gradually coats the material with a paint film through the spherical accompanying plating material that is constantly in contact with the material. This process is efficient, has less waste of resources, and the obtained coating film has a uniform thickness, so it has great room for development. Epoxy paint is often used in the roller spraying process, but conventional epoxy paint has limited chemical resistance (corrosion resistance), and most of them are solvent-based paints, which are highly polluting. Moreover, because parts are prone to adhesion during the roller spraying process of conventional epoxy coatings, they can only be roller sprayed for a while, then taken out for curing, then put into the roller spray machine for spraying, and then taken out for curing. This method must be repeated 3 to 6 times to achieve the required film thickness (the chemical resistance requirements are met through a certain film thickness, so the coating film thickness is higher). The film thickness requirements cannot be achieved with a single spraying, the spraying efficiency is low, and it is time-consuming and labor-intensive.

[0003] Therefore, developing a special roller spray coating for small-sized NdFeB magnets is the main technical problem that needs to be solved at present and has great economic value. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a water-based roller spray coating and a preparation method and application thereof to improve the workability and chemical resistance.

[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0006] A water-based roller spray paint, wherein the raw materials for its preparation include the following components by weight: 30-45 parts of a first water-based epoxy resin, 10-15 parts of a second water-based epoxy resin, 1-2 parts of a dispersant, 1-20 parts of water, 5-10 parts of a filler, 0.1-0.5 parts of a pH regulator, and 3-5 parts of an amino resin;

[0007] The epoxy equivalent of the first waterborne epoxy resin is 900 to 1060 g / mol;

[0008] The second waterborne epoxy resin is a bisphenol A type epoxy resin modified by a reactive emulsifier, and its epoxy equivalent is 520 to 600 g / Eq.

[0009] As a further improvement, the raw materials for its preparation also include: 10 to 20 parts of color paste, 0.2 to 0.5 parts of defoaming agent, 1 to 2 parts of wetting agent, 5 to 10 parts of film-forming aid, and 3 to 5 parts of adhesion promoter.

[0010] As a further improvement, the viscosity of the first waterborne epoxy resin is 200-6000 cP, and the solid content is 52±2%.

[0011] As a further improvement, the first water-based epoxy resin adopts JT-WBE522 of Polyco Technology.

[0012] As a further improvement, the second water-based epoxy resin adopts E-pos1011W55 from QR-Polymers.

[0013] As a further improvement, the filler is talcum powder.

[0014] As a further improvement, the pH adjuster is an amine neutralizer.

[0015] The method for preparing the water-based roller spray coating provided by the present invention comprises the following steps:

[0016] Adding the defoamer, wetting agent and film-forming aid into the first waterborne epoxy resin and the second waterborne epoxy resin under stirring and mixing them evenly;

[0017] Add dispersant and filler under stirring and mix well;

[0018] Add color paste, amino resin and adhesion promoter under stirring and mix well;

[0019] Add pre-mixed deionized water and pH adjuster, disperse evenly and filter to obtain water-based roller spray paint.

[0020] The application of the water-based roller spray paint provided by the present invention is to apply the water-based roller spray paint on a material by roller spraying, and then bake to obtain a dry film.

[0021] As a further improvement, the single roll spraying is performed to a film thickness of 5 to 15 μm.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The water-based roller spray coating of the present invention can be applied to small-sized NdFeB magnetic steel materials, has good construction performance, stable oil output during the spraying process, and no adhesion between materials with a maximum single spray thickness of 40 μm or more. Compared with multiple roller sprayings to achieve the target film thickness, it greatly saves production time.

[0024] (2) The coating of the present invention requires a low film thickness, with a minimum of 5 μm being sufficient to meet the performance test requirements, and a single roll coating can achieve a target film thickness of 5 to 15 μm.

[0025] (3) The coating of the present invention has excellent chemical resistance, and only a paint film of 5 μm thickness is required to pass the oleic acid immersion test for 72 hours under high temperature and high humidity conditions (temperature 65° C., humidity 90%).

[0026] (4) The coating of the present invention adopts a water-based system, with a theoretically calculated VOC of less than 300 g / L, less organic solvent volatilization, and meets environmental protection requirements. DETAILED DESCRIPTION

[0027] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0028] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0029] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0030] In some specific embodiments, the water-based roller spray coating of the present invention comprises the following components in parts by weight: 30 to 45 parts of a first water-based epoxy resin, 10 to 15 parts of a second water-based epoxy resin, 10 to 20 parts of a color paste, 0.2 to 0.5 parts of a defoaming agent, 1 to 2 parts of a wetting agent, 1 to 2 parts of a dispersant, 1 to 20 parts of water, 5 to 10 parts of a filler, 5 to 10 parts of a film-forming aid, 0.1 to 0.5 parts of a pH adjuster, 3 to 5 parts of an amino resin, and 3 to 5 parts of an adhesion promoter.

[0031] The epoxy equivalent of the first waterborne epoxy resin is 900-1060 g / mol, the viscosity is preferably 200-6000 cP, and the solid content is preferably 52±2%. Specifically, JT-WBE522 of Polyco Technology can be used. It has excellent shear stability and abrasion resistance, fast drying, excellent initial water resistance and other characteristics.

[0032] The second waterborne epoxy resin is a bisphenol A epoxy resin modified by a reactive emulsifier, and its epoxy equivalent (solid state) is 520-600 g / Eq; the solid content is preferably 51-55%. Specifically, E-pos1011W55 produced by QR-Polymers can be used. It has good corrosion resistance on multiple substrates.

[0033] In the prior art, it is difficult to achieve good oleic acid resistance. The present invention uses two specific water-based epoxy resins to compound, which significantly improves chemical resistance and takes into account adhesion and workability. The first or second water-based epoxy resin alone has poor chemical resistance, and the oleic acid and salt spray tests are NG. The second water-based epoxy resin also has adhesion and workability problems when used alone.

[0034] In some embodiments, the color paste used in the present invention is a black paste with a solid content of 35wt%, which is made by grinding high-pigment carbon black. It has good compatibility with the system, does not float color 3 months after being made into a colored paint, has good hiding power, and can completely cover the material when the paint film is 5μm.

[0035] In some embodiments, the defoaming agent used in the present invention is one or more of polyether siloxane copolymers and polydimethylsiloxanes, specifically one or more of tego902W from Tego and BYK024 from BYK.

[0036] In some embodiments, the wetting agent used in the present invention is an organosiloxane surfactant developed based on Gemini technology, which has excellent anti-oil and anti-crater capabilities, specifically Greesol GS195 from Yueyang Kaimen.

[0037] In some embodiments, the dispersant used in the present invention is one or more of a high molecular weight block copolymer solution, a copolymer containing a pigment affinity group, and an organic modified polyacrylate solution containing a pigment affinity group. The dispersant is used to disperse the matting powder so that the prepared coating has strong uniformity, is fine and does not bloom. Specifically, it is one or more of BYK2012 and BYK2013;

[0038] In some embodiments, the filler used in the present invention is talcum powder, specifically 3000 mesh ultrafine talcum powder produced by Guangdong Shenpeng Powder Material Co., Ltd.

[0039] In some embodiments, the film-forming aid used in the present invention is DPNB.

[0040] In some embodiments, the pH adjuster used in the present invention is an amine neutralizer, which mainly adjusts the pH of the coating to a weakly alkaline range, is beneficial to the storage of water-based coatings, improves activation and prevents sedimentation, etc., specifically DMEA.

[0041] In some embodiments, the amino resin used in the present invention is a crosslinking agent containing isobutyl alcohol methyl etherified high imino melamine, specifically CYMEL 325 from Allnex.

[0042] In some embodiments, the adhesion promoter used in the present invention is 3-glycidyl ether propyl trimethoxy silane, which mainly forms a chemical bond between the coating and the surface of the material through the active organic epoxy group and the hydrolyzable methoxy silane group to achieve the effect of improving adhesion, specifically, evonik GLYMO.

[0043] In some specific embodiments, the method for preparing the water-based roller spray coating of the present invention comprises:

[0044] Adding the defoamer, wetting agent and film-forming aid into the first waterborne epoxy resin and the second waterborne epoxy resin under stirring and mixing them evenly;

[0045] Add dispersant and filler under stirring and mix well;

[0046] Add color paste, amino resin and adhesion promoter under stirring and mix well;

[0047] Add pre-mixed deionized water and pH adjuster, disperse evenly and filter to obtain water-based roller spray paint.

[0048] In some specific embodiments, the construction method of the water-based roller spray coating of the present invention is: coating on the material by roller spraying, with a film thickness of 5 to 15 μm, and baking at 120 to 180° C. to obtain a dry film.

[0049] The product of the present invention is a water-based roller spray coating with excellent chemical resistance, but is not limited to roller spraying, and is also suitable for other methods such as automatic line spraying.

[0050] Embodiment and comparative example:

[0051] The raw materials and weights of the water-based roller spray coatings of Examples 1 to 4 and Comparative Examples 1 to 4 are shown in Tables 1 and 2. Among them, the first water-based epoxy resin is JT-WBE522 of Polyco Technology, the second water-based epoxy resin is E-pos 1011W55 of QR-Polymers, the black paste solid content is 35wt%, the defoamer is tego902W of Digo, the wetting agent is Greesol GS195 of Yueyang Kaimen, the dispersant is BYK2012 of BYK, the filler is 3000 mesh ultrafine talc powder of Guangdong Shenpeng Powder Material Company, the film-forming aid is DPNB, the pH adjuster is DMEA, the amino resin is CYMEL325 of allnex, and the adhesion promoter is evonik GLYMO.

[0052] The preparation method of the water-based roller spray coating of Examples 1 to 4 and Comparative Examples 1 to 4 is as follows:

[0053] S1, adding the first waterborne epoxy resin and the second waterborne epoxy resin in the components into a dispersion container;

[0054] S2. Add defoamer, wetting agent and film-forming agent at 600-800 rpm and stir for 5-8 minutes;

[0055] S3. Increase the speed to 800-1000 rpm, add dispersant and filler, stir at high speed for 10-20 minutes, and pay attention to scraping the edges. Pay attention to cooling during the process;

[0056] S4. Reduce the speed to 600-8000 rpm, add color paste, amino resin and adhesion promoter, and stir for 3-5 minutes;

[0057] S5. Add deionized water and pH regulator. Mix the deionized water and pH regulator in advance and let them stand for more than 5 minutes at room temperature before adding. Use pH regulator to adjust pH and deionized water to adjust viscosity (temperature is controlled at 5-35°C throughout the process).

[0058] S6. Filter the package with a 250-350 mesh filter to obtain the water-based roller spray paint.

[0059] Table 1 Components and weight parts of the examples

[0060]

[0061]

[0062] Table 2 Comparative Examples Components and Weight Parts

[0063]

[0064]

[0065] Performance Testing:

[0066] Construction method: Add water to the water-based roller spray coating prepared in the above Examples 1 to 4 and Comparative Examples 1 to 4 to adjust the viscosity to a suitable construction, and apply it on the material by roller spraying. The thickness of a single roller coating is 5 to 15 μm, and the dry film with the final effect is obtained after baking at 150°C for 30 minutes. The performance test items are shown in Table 3:

[0067] Table 3 Performance test results

[0068]

[0069]

[0070] It can be seen that Examples 1 to 4 have excellent chemical resistance (oleic acid, salt spray), adhesion and workability. Comparative Examples 1 to 2 do not add the first water-based epoxy resin, and have poor chemical resistance (oleic acid and salt spray test NG), poor adhesion and workability. Comparative Examples 3 to 4 do not add the second water-based epoxy resin, and have poor chemical resistance (oleic acid and salt spray test NG).

[0071] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the scope of protection of the technical solution of the present invention.

Claims

1. A water-based spray coating, characterized in that: The raw materials for its preparation include the following components by weight: 30-45 parts of a first waterborne epoxy resin, 10-15 parts of a second waterborne epoxy resin, 1-2 parts of a dispersant, 1-20 parts of water, 5-10 parts of a filler, 0.1-0.5 parts of a pH regulator, and 3-5 parts of an amino resin; The epoxy equivalent of the first waterborne epoxy resin is 900 to 1060 g / mol; The second waterborne epoxy resin is a bisphenol A type epoxy resin modified by a reactive emulsifier, and its epoxy equivalent is 520 to 600 g / Eq.

2. The water-based roller spray paint according to claim 1, characterized in that: The raw materials for its preparation also include: 10 to 20 parts of color paste, 0.2 to 0.5 parts of defoaming agent, 1 to 2 parts of wetting agent, 5 to 10 parts of film-forming aid, and 3 to 5 parts of adhesion promoter.

3. The water-based roller spray paint according to claim 1 or 2, characterized in that: The first waterborne epoxy resin has a viscosity of 200-6000 cP and a solid content of 52±2%.

4. The water-based roller spray paint according to claim 1 or 2, characterized in that: The first water-based epoxy resin is JT-WBE522 from Polyco Technology.

5. The water-based roller spray paint according to claim 1 or 2, characterized in that: The second water-based epoxy resin is E-pos 1011W55 from QR-Polymers.

6. The water-based roller spray paint according to claim 1 or 2, characterized in that: The filler is talc.

7. The water-based roller spray paint according to claim 1, characterized in that: The pH adjuster is an amine neutralizer.

8. A method for preparing the water-based roller spray coating according to any one of claims 1 to 7, characterized in that: The steps include: Adding the defoamer, wetting agent and film-forming aid into the first waterborne epoxy resin and the second waterborne epoxy resin under stirring and mixing them evenly; Add dispersant and filler under stirring and mix well; Add color paste, amino resin and adhesion promoter under stirring and mix well; Add pre-mixed deionized water and pH adjuster, disperse evenly and filter to obtain water-based roller spray paint.

9. An application of the water-based roller spray paint according to any one of claims 1 to 7, characterized in that: The water-based roller spray paint is applied on the material by roller spraying, and then baked to obtain a dry film.

10. The use according to claim 9, characterized in that: Roll spray once to a film thickness of 5 to 15 μm.

Citation Information

Patent Citations

  • Water-borne rolling and spraying puller paint and preparation method and application thereof

    CN107236427A

  • Water-based paint as well as preparation method and application thereof

    CN117487430A

  • Aqueous coating composition, coated film and article

    JP2024092858A

  • Two-component aqueous epoxy resin paint

    US20220106494A1