Water-based paint for automobile compartment and preparation method thereof
By using nano-calcium carbonate and graphene oxide in water-based automotive paints, a highly oriented cross-linked structure of activated graphene and water-based polyurethane is formed, which solves the problems of corrosion and impact damage of existing water-based paints and achieves high resistance The improvement of scratch and corrosion resistance meets environmental protection requirements.
Patent Information
- Application Number
- CN202411249377.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-06
AI Technical Summary
Existing water-based automotive paints are susceptible to corrosion and impact damage caused by corrosive media during long-term use, and cannot meet the needs of scratch resistance and corrosion resistance.
Using aqueous polyurethane as the resin component, combined with nano calcium carbonate, graphene oxide, end amino polyamide, chitosan, defoaming agent, leveling agent and dispersant, through specific stirring, sonication and freeze-drying steps, Highly oriented activated graphene is formed and crosslinked with aqueous polyurethane to form a three-dimensional network structure to enhance the impact strength and wear resistance of the coating.
It significantly improves the impact strength, scratch resistance and corrosion resistance of the coating, enhances the adhesion with metal substrates, reduces the VOC content, meets environmental protection requirements, and improves the service life and quality of the product.
Smart Images

Figure CN118755374B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based paint for vehicles, and in particular to a water-based paint for automobile compartments and a preparation method thereof. Background Art
[0002] As people's awareness of environmental protection and energy increases, environmental protection laws and regulations of various countries strictly limit the content of volatile organic compounds in paint systems, which promotes the development of water-based paint. Automotive paint generally refers to paint for new cars and auxiliary materials and paint for vehicle repair. With the continuous growth of the number of cars in my country, it provides a huge market development space for my country's automotive water-based paint industry, and the amount of automotive paint also shows a rising trend.
[0003] Water-based car paint often uses water-based polyurethane as the resin component. The polyurethane paint coating has the characteristics of impact resistance, corrosion resistance, chemical resistance and good wear resistance, and has been widely used in car compartments. However, after long-term use, corrosive media can easily penetrate into the coating and accelerate the shedding of the coating, causing corrosion of the substrate. At the same time, when the road environment is relatively harsh, the car is easily impacted by flying stones or debris while driving, and the coating will be damaged and peeled off due to the impact, which cannot meet people's demand for car paint.
[0004] Therefore, further research is needed on water-based automotive paint. How to overcome the shortcomings of the existing technology and prepare a water-based automotive paint that can enhance impact strength, scratch resistance and corrosion resistance has become an urgent problem to be solved in the coating field. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a water-based paint for automobile compartments and a preparation method thereof.
[0006] A water-based paint for automobile compartments comprises the following raw materials by mass: 50-150 parts of water-based polyurethane, 10-20 parts of nano calcium carbonate, 1-5 parts of graphene oxide, 1-2 parts of amino-terminated polyamidoamine, 1-2 parts of chitosan, 1-2 parts of defoamer, 1-2 parts of leveling agent, 1-2 parts of dispersant and 50-100 parts of water.
[0007] Preferably, the particle size of nano calcium carbonate is 20-50 nm.
[0008] Preferably, the graphene oxide has a sheet diameter of 0.5-5 μm and a thickness of 0.8-1.2 nm.
[0009] Preferably, the defoamer is a silicone defoamer, preferably a polyether-modified silicone defoamer.
[0010] Preferably, the leveling agent is an aralkylsiloxane leveling agent.
[0011] Preferably, the dispersant is a fatty alcohol ether phosphate.
[0012] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0013] S1. Add graphene oxide and amino-terminated polyamidoamine to water, stir at room temperature for 10-20 min, heat to 80-90° C., stir for 1-2 h, filter, and vacuum dry to obtain pretreated graphene;
[0014] S2, adding chitosan to the acetic acid aqueous solution and stirring evenly, mixing with the pretreated graphene, ultrasonically treating for 1-2 hours, hydrothermally treating at 180-220° C. for 10-20 hours, cooling, sending to a container with a cold source at the bottom, directionally freezing to -30 to -50° C., standing for 1-2 hours, and freeze-drying to obtain activated graphene;
[0015] S3. Mix waterborne polyurethane, activated graphene, nano calcium carbonate and water, then add defoamer, leveling agent and dispersant and continue stirring.
[0016] Preferably, in S2, the mass fraction of the acetic acid aqueous solution is 1-1.5%.
[0017] Preferably, in S2, the ultrasonic frequency is 10-15 kHz, and the ultrasonic temperature is 40-50°C. Beneficial Effects
[0018] 1. Since there are a large number of epoxy groups at the edge of graphene oxide, the present invention utilizes the ring opening of epoxy groups of graphene oxide sheets and reacts with the amine groups of terminal amino polyamide amine, so that the sheet structure is coated with dendritic macromolecules and forms a regular distribution of organic and inorganic. This can not only effectively solve the problem that graphene sheets are easy to agglomerate, but also generate directional force through filtration to promote the highly ordered arrangement of the sheet structure, and cooperate with chitosan for cross-linking to form a hydrogel structure. After a specific freezing treatment, ice crystals grow upward along the temperature gradient direction to ensure a highly ordered pore size, which has good compatibility with water-based polyurethane and significantly improves the impact strength and wear resistance of the coating.
[0019] 2. The activated graphene obtained by the present invention has a high degree of orientation, large porosity and specific surface area, and forms a three-dimensional network structure with polyurethane. It is not only stable in storage at room temperature, but also has excellent scratch resistance after curing. At the same time, it can improve the adhesion of the coating to the substrate, especially enhance the interaction with the metal substrate, effectively inhibit the occurrence of electrochemical corrosion, and improve its corrosion resistance.
[0020] 3. The present invention significantly enhances the crosslinking between inorganic and organic substances while achieving water dispersibility and storage stability of graphene and nano-calcium carbonate in water-based resin. At the same time, the coating obtained by the present invention has good surface gloss, strong adhesion, good storage stability, and wear resistance, thereby improving the quality and service life of the product.
[0021] 4. The VOC content of the present invention is low, which meets the environmental protection requirements of automobile coatings and has no pungent odor. At the same time, it is simple to prepare, easy to paint, has a small coating thickness, and has a good light retention rate, and can be widely used in automobile painting. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 N is the N of the activated graphene obtained in Example 5 2 Adsorption-desorption isotherms.
[0023] Figure 2 It is a comparison chart of the corrosion potential and impact strength of the coatings obtained in Example 5 and Comparative Examples 1-3.
[0024] Figure 3 The figure is a comparison chart of dry / wet scratch resistance of the coatings obtained in Example 5 and Comparative Examples 1-3.
[0025] Figure 2 and Figure 3 In the figure, the vertical line segment at the top of the column is the error bar, which represents the standard deviation of multiple test results. DETAILED DESCRIPTION
[0026] The present invention will be further explained below in conjunction with specific embodiments.
[0027] The water-based polyurethane used below was purchased from Qingdao Kos New Material Technology Co., Ltd., model FS-108C. The polyether-modified silicone defoamer used below was purchased from Dongguan Zhongxin Material Research Institute Co., Ltd. The BYK323 used below was purchased from Shenzhen Chengtai Trading Co., Ltd. The fatty alcohol ether phosphate MOA-9P used below was purchased from Jiangsu An Petrochemical Plant. Example 1
[0028] A water-based paint for automobile compartments comprises raw materials: 500 g of water-based polyurethane, 100 g of nano-calcium carbonate with a particle size of 20-50 nm, 10 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 10 g of amino-terminated polyamidoamine, 10 g of chitosan, 10 g of polyether-modified silicone defoamer, 10 g of BYK323, 10 g of fatty alcohol ether phosphate MOA-9P, and 500 g of water.
[0029] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0030] S1, adding graphene oxide and amino-terminated polyamidoamine to 200g of water, stirring at room temperature at a speed of 1000r / min for 10min, heating to 80°C and stirring for 1h, filtering, and vacuum drying to obtain pretreated graphene;
[0031] S2, adding chitosan to 100g of 1% acetic acid aqueous solution, stirring evenly, mixing with pretreated graphene, ultrasonically treating for 1h, the ultrasonic frequency is 10kHz, the ultrasonic temperature is 40°C, sending it into a hydrothermal reactor lined with polytetrafluoroethylene, hydrothermally treating it at a temperature of 180°C for 10h, cooling it, sending it into a container with a cold source at the bottom, directionally freezing it to -30°C, standing it for 1h, and freeze-drying it to obtain activated graphene;
[0032] S3. Mix waterborne polyurethane, activated graphene, nano-calcium carbonate and water, stir at a speed of 1000 r / min for 10 min, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 1 h, and degas. Example 2
[0033] A water-based paint for automobile compartments comprises raw materials: 1500 g of water-based polyurethane, 200 g of nano calcium carbonate with a particle size of 20-50 nm, 50 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 20 g of amino-terminated polyamidoamine, 20 g of chitosan, 20 g of polyether-modified silicone defoamer, 20 g of BYK323, 20 g of fatty alcohol ether phosphate MOA-9P, and 1000 g of water.
[0034] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0035] S1, adding graphene oxide and amino-terminated polyamidoamine to 400g water, stirring at room temperature at a speed of 2000r / min for 20min, heating to 90°C and stirring for 2h, filtering, and vacuum drying to obtain pretreated graphene;
[0036] S2, adding chitosan to 200g of acetic acid aqueous solution with a mass fraction of 1.5%, stirring evenly, mixing with pretreated graphene, ultrasonically treating for 2h, the ultrasonic frequency is 15kHz, the ultrasonic temperature is 50°C, sending it into a hydrothermal reactor lined with polytetrafluoroethylene, hydrothermally treating it at a temperature of 220°C for 20h, cooling it, sending it into a container with a cold source at the bottom, directionally freezing it to -50°C, standing it for 2h, and freeze-drying it to obtain activated graphene;
[0037] S3. Mix waterborne polyurethane, activated graphene, nano-calcium carbonate and water, stir at 2000 r / min for 20 min, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 2 h, and degas. Example 3
[0038] A water-based paint for automobile compartments comprises raw materials: 800 g of water-based polyurethane, 180 g of nano-calcium carbonate with a particle size of 20-50 nm, 20 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 18 g of amino-terminated polyamidoamine, 13 g of chitosan, 18 g of polyether-modified silicone defoamer, 13 g of BYK323, 18 g of fatty alcohol ether phosphate MOA-9P, and 700 g of water.
[0039] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0040] S1, adding graphene oxide and amino-terminated polyamidoamine to 350g water, stirring at room temperature at a speed of 1200r / min for 17min, heating to 82°C and stirring for 100min, filtering, and vacuum drying to obtain pretreated graphene;
[0041] S2, adding chitosan to 120g of acetic acid aqueous solution with a mass fraction of 1.3%, stirring evenly, mixing with pretreated graphene, ultrasonically treating for 80min, the ultrasonic frequency is 13kHz, the ultrasonic temperature is 43°C, sending it into a hydrothermal reactor lined with polytetrafluoroethylene, hydrothermally treating it at a temperature of 210°C for 12h, cooling it, sending it into a container with a cold source at the bottom, directionally freezing it to -45°C, standing it for 80min, and freeze-drying it to obtain activated graphene;
[0042] S3. Mix waterborne polyurethane, activated graphene, nano-calcium carbonate and water, stir at a speed of 1700 r / min for 12 min, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 100 min, and degas. Example 4
[0043] A water-based paint for automobile compartments comprises raw materials: 1200 g of water-based polyurethane, 120 g of nano calcium carbonate with a particle size of 20-50 nm, 40 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 12 g of amino-terminated polyamidoamine, 17 g of chitosan, 12 g of polyether-modified silicone defoamer, 17 g of BYK323, 12 g of fatty alcohol ether phosphate MOA-9P, and 900 g of water.
[0044] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0045] S1, adding graphene oxide and amino-terminated polyamidoamine to 250g of water, stirring at room temperature at a speed of 1800r / min for 13min, heating to 88°C and stirring for 80min, filtering, and vacuum drying to obtain pretreated graphene;
[0046] S2, adding chitosan to 180g of acetic acid aqueous solution with a mass fraction of 1.1%, stirring evenly, mixing with pretreated graphene, ultrasonically treating for 100min, the ultrasonic frequency is 11kHz, the ultrasonic temperature is 47°C, sending it into a hydrothermal reactor lined with polytetrafluoroethylene, hydrothermally treating it at a temperature of 190°C for 18h, cooling it, sending it into a container with a cold source at the bottom, directionally freezing it to -35°C, standing it for 100min, and freeze-drying it to obtain activated graphene;
[0047] S3. Mix waterborne polyurethane, activated graphene, nano-calcium carbonate and water, stir at a speed of 1300 r / min for 18 min, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 80 min, and degas. Example 5
[0048] A water-based paint for automobile compartments comprises raw materials: 1000 g of water-based polyurethane, 150 g of nano-calcium carbonate with a particle size of 20-50 nm, 30 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 15 g of amino-terminated polyamidoamine, 15 g of chitosan, 15 g of polyether-modified silicone defoamer, 15 g of BYK323, 15 g of fatty alcohol ether phosphate MOA-9P, and 800 g of water.
[0049] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0050] S1, adding graphene oxide and amino-terminated polyamidoamine to 300g water, stirring at room temperature at a speed of 1500r / min for 15min, heating to 85°C and stirring for 90min, filtering, and vacuum drying to obtain pretreated graphene;
[0051] S2, adding chitosan to 150g of acetic acid aqueous solution with a mass fraction of 1.2%, stirring evenly, mixing with pretreated graphene, ultrasonically treating for 90min, the ultrasonic frequency is 12kHz, the ultrasonic temperature is 45°C, sending it into a hydrothermal reactor lined with polytetrafluoroethylene, hydrothermally treating it at a temperature of 200°C for 15h, cooling it, sending it into a container with a cold source at the bottom, directionally freezing it to -40°C, standing it for 90min, and freeze-drying it to obtain activated graphene;
[0052] The activated graphene obtained above was subjected to adsorption and desorption tests using nitrogen. 2 Adsorption-desorption isotherms. Figure 1 As shown, the activated graphene obtained in this embodiment has a high specific surface area, a suitable pore structure and sufficient pore volume.
[0053] S3. Mix waterborne polyurethane, activated graphene, nano-calcium carbonate and water, stir at a speed of 1500 r / min for 15 minutes, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 90 minutes, and degas.
[0054] Comparative Example 1
[0055] A water-based paint for automobile compartments comprises raw materials: 1000 g of water-based polyurethane, 150 g of nano calcium carbonate with a particle size of 20-50 nm, 30 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 15 g of amino-terminated polyamidoamine, 15 g of polyether-modified silicone defoamer, 15 g of BYK323, 15 g of fatty alcohol ether phosphate MOA-9P, and 800 g of water.
[0056] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0057] S1, adding graphene oxide and amino-terminated polyamidoamine to 300g water, stirring at room temperature at a speed of 1500r / min for 15min, heating to 85°C and stirring for 90min, filtering, and vacuum drying to obtain pretreated graphene;
[0058] S2. Mix waterborne polyurethane, pretreated graphene, nano-calcium carbonate and water, stir at a speed of 1500 r / min for 15 min, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 90 min, and degas.
[0059] Comparative Example 2
[0060] A water-based paint for automobile compartments comprises raw materials: 1000 g of water-based polyurethane, 150 g of nano-calcium carbonate with a particle size of 20-50 nm, 30 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 15 g of amino-terminated polyamidoamine, 15 g of chitosan, 15 g of polyether-modified silicone defoamer, 15 g of BYK323, 15 g of fatty alcohol ether phosphate MOA-9P, and 800 g of water.
[0061] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0062] S1, adding graphene oxide and amino-terminated polyamidoamine to 300g water, stirring at room temperature at a speed of 1500r / min for 15min, heating to 85°C and stirring for 90min, and vacuum drying to obtain pretreated graphene;
[0063] S2, adding chitosan to 150g of acetic acid aqueous solution with a mass fraction of 1.2%, stirring evenly, mixing with pretreated graphene, ultrasonically treating for 90min, the ultrasonic frequency is 12kHz, the ultrasonic temperature is 45°C, sending it into a hydrothermal reactor lined with polytetrafluoroethylene, hydrothermally treating it at a temperature of 200°C for 15h, cooling it, sending it into a container with a cold source at the bottom, directionally freezing it to -40°C, standing it for 90min, and freeze-drying it to obtain activated graphene;
[0064] S3. Mix waterborne polyurethane, activated graphene, nano-calcium carbonate and water, stir at a speed of 1500 r / min for 15 minutes, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 90 minutes, and degas.
[0065] Comparative Example 3
[0066] A water-based paint for automobile compartments comprises raw materials: 1000 g of water-based polyurethane, 150 g of nano-calcium carbonate with a particle size of 20-50 nm, 30 g of graphene oxide with a sheet size of 0.5-5 μm and a thickness of 0.8-1.2 nm, 15 g of amino-terminated polyamidoamine, 15 g of chitosan, 15 g of polyether-modified silicone defoamer, 15 g of BYK323, 15 g of fatty alcohol ether phosphate MOA-9P, and 800 g of water.
[0067] The method for preparing the water-based paint for automobile compartments comprises the following steps:
[0068] S1, adding graphene oxide and amino-terminated polyamidoamine to 300g water, stirring at room temperature at a speed of 1500r / min for 15min, heating to 85°C and stirring for 90min, filtering, and vacuum drying to obtain pretreated graphene;
[0069] S2, adding chitosan to 150g of acetic acid aqueous solution with a mass fraction of 1.2%, stirring evenly, mixing with pretreated graphene, ultrasonically treating for 90min, with an ultrasonic frequency of 12kHz and an ultrasonic temperature of 45°C, sending it into a hydrothermal reactor lined with polytetrafluoroethylene, hydrothermally treating it at a temperature of 200°C for 15h, cooling it, and freeze-drying it to obtain activated graphene;
[0070] S3. Mix waterborne polyurethane, activated graphene, nano-calcium carbonate and water, stir at a speed of 1500 r / min for 15 minutes, then add polyether modified silicone defoamer, BYK323 and fatty alcohol ether phosphate MOA-9P, continue stirring for 90 minutes, and degas.
[0071] The water-based paint obtained in Example 5 and Comparative Examples 1-3 was uniformly sprayed on tinplate, and the coating thickness was 30±5 μm, and baked at 60° C. for 30 min to obtain coating samples. The performance of each group of coating samples was then tested, as follows:
[0072] (1) Refer to GB / T 9286-2021 "Scratch test for paints and varnishes" to test the adhesion grade of each group of coating samples.
[0073] (2) Refer to GB / T 6739-2022 “Determination of film hardness of paints and varnishes - pencil method” to test the hardness of each group of coating samples.
[0074] (3) Test each group of coating samples with reference to GB / T 1733-1993 “Determination of water resistance of paint films”.
[0075] (4) Electrochemical tests were performed on each group of coating samples using an electrochemical workstation. A three-electrode system was used, with a saturated calomel electrode as the reference electrode, a platinum electrode as the auxiliary electrode, a film sample as the working electrode, and a 3.5% by mass NaCl aqueous solution as the electrolyte.
[0076] (5) Test each group of coating samples with reference to GB / T 1732-2020 “Determination of impact resistance of paint films”.
[0077] (6) Dry scratch resistance: A thin layer of BonAmi abrasive was applied to the coating surface of each group of coating samples. Then, a color-matching felt fingertip was put on and the sample plate was touched and rubbed back and forth 10 times. The relative gloss ratio of the scratched area to the unscratched area at a viewing angle of 20 degrees (i.e., the gloss retention percentage) was measured.
[0078] (7) Wet scratch resistance: Wet alumina slurry [alumina (120# angular sand) 2.02%, AMP-95 aqueous solution 7.20%, ASE-60 thickener 6.05%, balance deionized water] was applied to the coating surface of each group of coating samples, and then a color-matching felt fingertip was put on and pressed against the contact sample plate. The fingertip was wiped back and forth 10 times, and the relative gloss ratio of the scratched area to the unscratched area of the sample at a viewing angle of 20 degrees (i.e., the gloss retention percentage) was measured.
[0079] The results are shown in the following table and Figure 2-Figure 3 shown.
[0080] All the results confirmed that the coating obtained in Example 5 had excellent adhesion, high hardness, good water resistance, high corrosion potential and impact strength, and excellent dry / wet scratch resistance, and all the results were better than the coatings obtained in Comparative Examples 1-3 (P < 0.05).
[0081] The applicant believes that this is because the present invention utilizes the ring opening of the epoxy group of the graphene oxide sheet and reacts with the amine group of the amino-terminated polyamide amine, so that the sheet structure is coated with dendritic macromolecules and forms a regular distribution of organic and inorganic molecules, which can not only effectively solve the problem that the graphene sheet is easy to agglomerate, but also the directional force generated by the suction filtration promotes the highly ordered arrangement of the sheet structure, and cooperates with chitosan to form a hydrogel structure for cross-linking. After a specific freezing treatment, the ice crystals grow upward along the temperature gradient direction to ensure a highly ordered pore size, which has good compatibility with water-based polyurethane and significantly improves the impact strength and wear resistance of the coating; at the same time, the activated graphene obtained by the present invention has a high degree of orientation, a large porosity and a large specific surface area, and forms a three-dimensional network structure with polyurethane, which is not only stable in storage at room temperature, but also has excellent scratch resistance after curing, and can improve the adhesion of the coating to the substrate, especially enhance the interaction with the metal substrate, effectively inhibit the occurrence of electrochemical corrosion, and improve its corrosion resistance.
[0082] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A water-based paint for automobile compartments, characterized in that: The raw materials include, by mass: 50-150 parts of waterborne polyurethane, 10-20 parts of nano calcium carbonate, 1-5 parts of graphene oxide, 1-2 parts of amino-terminated polyamide amine, 1-2 parts of chitosan, 1-2 parts of defoamer, 1-2 parts of leveling agent, 1-2 parts of dispersant, and 50-100 parts of water; Prepared by the following steps: S1. Add graphene oxide and amino-terminated polyamidoamine to water, stir at room temperature for 10-20 min, heat to 80-90° C., stir for 1-2 h, filter, and vacuum dry to obtain pretreated graphene; S2, adding chitosan to the acetic acid aqueous solution and stirring evenly, mixing with the pretreated graphene, ultrasonically treating for 1-2 hours, hydrothermally treating at 180-220° C. for 10-20 hours, cooling, sending to a container with a cold source at the bottom, directionally freezing to -30 to -50° C., standing for 1-2 hours, and freeze-drying to obtain activated graphene; S3. Mix water-based polyurethane, activated graphene, nano calcium carbonate and water, then add defoamer, leveling agent and dispersant and continue stirring.
2. The water-based paint for automobile compartments according to claim 1, characterized in that: The particle size of nano calcium carbonate is 20-50nm.
3. The water-based paint for automobile compartment according to claim 1, characterized in that: The sheet diameter of graphene oxide is 0.5-5 μm and the thickness is 0.8-1.2 nm.
4. The water-based paint for automobile compartment according to claim 1, characterized in that: The defoaming agent is a silicone defoaming agent.
5. The water-based paint for automobile compartment according to claim 1, characterized in that: The defoaming agent is a polyether modified silicone defoaming agent.
6. The water-based paint for automobile compartment according to claim 1, characterized in that: The leveling agent is an aromatic siloxane leveling agent.
7. The water-based paint for automobile compartments according to claim 1, characterized in that: The dispersant is fatty alcohol ether phosphate.
8. A method for preparing a water-based paint for automobile compartments as claimed in any one of claims 1 to 7, characterized in that: The steps include: S1. Add graphene oxide and amino-terminated polyamidoamine to water, stir at room temperature for 10-20 min, heat to 80-90° C., stir for 1-2 h, filter, and vacuum dry to obtain pretreated graphene; S2, adding chitosan to the acetic acid aqueous solution and stirring evenly, mixing with the pretreated graphene, ultrasonically treating for 1-2 hours, hydrothermally treating at 180-220° C. for 10-20 hours, cooling, sending to a container with a cold source at the bottom, directionally freezing to -30 to -50° C., standing for 1-2 hours, and freeze-drying to obtain activated graphene; S3. Mix water-based polyurethane, activated graphene, nano calcium carbonate and water, then add defoamer, leveling agent and dispersant and continue stirring.
9. The method for preparing water-based paint for automobile compartment according to claim 8, characterized in that: In S2, the mass fraction of the acetic acid aqueous solution is 1-1.5%.
10. The method for preparing water-based paint for automobile compartment according to claim 8, characterized in that: In S2, the ultrasonic frequency is 10-15 kHz and the ultrasonic temperature is 40-50°C.