Thermochromic layer, preparation method of thermochromic layer, insulating material and preparation method of insulating material
The thermochromic layer and high surface flashover strength top layer prepared by mixing cholesteric liquid crystal and alkanol solve the problem of temperature change monitoring and performance improvement of insulating materials, and achieve real-time temperature display and performance improvement of insulating materials.
Patent Information
- Application Number
- CN202410889676.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-11
AI Technical Summary
Insulation defects inevitably occur in existing insulation materials during use, causing temperature rise and affecting insulation performance. Moreover, there is a lack of intuitive surface temperature measurement methods, making it difficult to monitor the insulation temperature changes of electrical equipment in real time.
The thermochromic layer is prepared by mixing cholesteric liquid crystal and alkanol, combined with the top layer of high surface flashover strength to form a double-layer insulating material. The thermochromic layer can show multi-color changes at different temperatures, visually display temperature changes, and pass The high surface flashover intensity top layer inhibits surface charge accumulation and improves surface flashover intensity.
It realizes real-time temperature monitoring of insulating materials, improves the insulation performance, especially remains stable under conditions of high humidity and mechanical stress, and has a simple preparation process, making it suitable for mass production.
Smart Images

Figure CN118755484A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional insulating material preparation, and in particular to a thermochromic layer and a preparation method thereof, and an insulating material and a preparation method thereof. Background Art
[0002] Insulation structure is an important part of power equipment, but insulation defects are inevitable during the manufacturing, installation and operation of equipment, causing insulation breakdown and surface flashover faults. Insulation defects refer to some abnormal structures that affect the insulation performance of the insulation materials of power equipment, including concentrated defects such as bubbles, cracks, local damage, electrode tips, foreign matter, and dispersed defects such as moisture and aging. These defects will affect the normal operation of electrical and electronic equipment. Insulation defects usually lead to an increase in local electric fields, causing discharge and temperature rise, causing the insulation material to age continuously and eventually causing insulation breakdown and other accidents, causing damage to power equipment and power outages in the power grid, seriously affecting the safe and stable operation of the power system.
[0003] At present, partial discharge measurement (ultrasound, ultra-high frequency, pulse current) and other methods are usually used to detect insulation defects. The partial discharge detection method detects the sound waves, electromagnetic waves, current and other signals generated during the operation of the equipment. It requires expensive and precise detection equipment, and requires the detection personnel to have rich professional knowledge. It lacks intuitiveness and universality, which limits its application to a certain extent. Insulation defects are usually accompanied by discharge and temperature rise. Introducing thermochromic materials into the insulation system can display the surface temperature of the material in real time and intuitively, becoming a new method for insulation defect detection. However, the color change principle of existing thermochromic insulation materials comes from the redox reaction of electron donors and electron acceptors, which can only achieve the depth change of a single color and it is difficult to accurately characterize the temperature change. Inspired by the biological stimulus-response characteristics in nature, cholesteric liquid crystal materials can make the coating color change reversibly with temperature, so as to realize the real-time and intuitive detection of the surface insulation temperature of electrical equipment.
[0004] CN112980248B discloses a thermochromic liquid crystal microcapsule ink, comprising the following mass fraction components: a first aqueous resin, a liquid crystal microcapsule, a first adhesion promoter, and a first curing agent, wherein: the liquid crystal microcapsule is mainly composed of a wall material and a core material, the core material mainly comprises a cholesteric phase liquid crystal, and the wall material is a polyurethane resin; and also relates to a thermochromic coating prepared from the above-mentioned thermochromic liquid crystal microcapsule ink. The thermochromic coating prepared from the reversible thermochromic liquid crystal microcapsule ink can be attached to different drinking containers, and the coating has excellent resistance to boiling, scratching, and chemicals, which can prevent the drinker from being scalded by hot water. The reversible color change of the cholesteric phase liquid crystal coating after heating directly reflects the change in temperature, and can monitor the temperature of the material in real time. The thermochromic ink in this technical solution requires the preparation of liquid crystal microcapsules, the preparation process is cumbersome, and it is difficult to ensure the uniformity of the microcapsule particle size, which affects the color change effect.
[0005] At the same time, choosing insulating materials with excellent insulation performance and avoiding insulation defects have become the development goals of insulating structures. Currently, the widely used insulating materials are organic polymers, including polyolefins, organic resins, and polyimides. Organic polymers have excellent mechanical, processing, and electrical properties, and are resistant to high temperatures, voltages, water, moisture, and corrosion, and are excellent in insulating materials. The bisphenol A structure in epoxy resin gives the polymer excellent toughness, rigidity, and high-temperature performance. The ether bonds and hydroxyl groups in epoxy resin are polar groups that can form strong interactions with a variety of surfaces and produce strong bonds. After curing, they can be widely used in high-voltage insulating parts, columnar insulating supports, etc. with inorganic particles.
[0006] CN113549301B discloses an epoxy resin ultra-high thermal conductive insulating material and a preparation method, wherein the material comprises an epoxy resin base material, a modified composite inorganic filler and a curing agent. Among them, the modified composite inorganic filler is composed of four inorganic fillers of different particle sizes. The technical scheme is to carry out surface modification and decontamination modification on the inorganic fillers of four particle sizes and then mix them, and select the particle size and the dosage ratio of different particle sizes, so that after the modified composite inorganic filler is mixed with the epoxy resin base material and the curing agent, its physical and electrical properties are maintained and it has the low viscosity characteristics required for the process implementation. The technical scheme does not consider the insulation properties such as breakdown strength. The high-content filler doping improves the thermal conductivity, but reduces the insulation performance; in addition, the high thermal conductive insulating material does not consider the thermochromic performance and cannot be used for the intuitive diagnosis of temperature.
[0007] In summary, insulation defects are inevitable during the use and installation of insulating materials, which will increase the temperature and lead to deterioration of insulation performance. Therefore, it is difficult to measure the surface temperature of insulating materials during use, and the poor electrical performance of insulating materials is still a problem that needs to be solved urgently. Summary of the invention
[0008] In view of the above problems, the present invention provides a thermochromic layer and a preparation method thereof and an insulating material and a preparation method thereof, wherein the thermochromic layer can present different colors at different temperatures, can intuitively display the surface temperature of the material, and the color change is reversible and can be used repeatedly; at the same time, an insulating material is prepared using the thermochromic layer, the insulating material comprises a matrix, a thermochromic layer and a top layer with high surface flashover strength, an alkane alcohol is added to the thermochromic layer, so that the thermochromic layer can adhere to the matrix in the insulating material and can interact with the epoxy resin in the top layer with high surface flashover strength, so that the color of the insulating material prepared in this way can change with temperature, and at the same time, the top layer with high surface flashover strength can inhibit surface charge accumulation, and has properties such as high surface flashover strength.
[0009] The invention provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.1-0.4 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10-60)±0.5°C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal comprises cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of (6-18): (1-13): 1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0010] Furthermore, the critical temperature of the thermochromic layer changes with the mass ratio (COC: CEP: CC) of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP), and cholesterol chloride (CC) as shown in Table 1.
[0011]
[0012] Furthermore, the mass ratio of the cholesteric liquid crystal to the alkanol is (1:1)-(2:1).
[0013] Furthermore, the alkanol is one or more of hexadecanol, nonadecanol, heneicosanol, hexacosanol, heptacosanol, octacosanol and triacontanol.
[0014] The present invention also provides a method for preparing the thermochromic layer, comprising the following steps: Cholesterol oleyl carbonate, cholesterol nonanoate, cholesterol chloride and alkanol are heated and stirred together in an oil bath to obtain a liquid crystal mixture, and the liquid crystal mixture is spin-coated into a film and cured to obtain the thermochromic layer.
[0015] Furthermore, the mass ratio of the total mass of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride to the mass ratio of the alkanol is (1:1)-(2:1).
[0016] Furthermore, the mass ratio of cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is (6-18):(1-13):1.
[0017] Furthermore, the alkanol is one or more of hexadecanol, nonadecanol, heneicosanol, hexacosanol, heptacosanol, octacosanol and triacontanol.
[0018] Furthermore, the heating and stirring temperature is 96-110° C., the heating and stirring speed is 800-1000 r / min, and the heating and stirring time is 1-2 h.
[0019] Furthermore, the rotation speed of the spin coating is 300-1200 r / min, and the spin coating time is 10-50 s.
[0020] Furthermore, the curing temperature is 60-120° C., and the curing time is 5-20 hours.
[0021] Furthermore, the thickness of the thermochromic layer is 0.1-0.4 mm.
[0022] The present invention also provides an insulating material comprising the thermochromic layer, wherein the insulating material is prepared from bottom to top in sequence from a matrix, the thermochromic layer and a top layer with high surface flashover strength; the color of the insulating material changes with its temperature, specifically: the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10-60) ± 0.5 ° C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is (10.2-20) ± 0.5 ° C, and the critical color change temperature from blue to purple is (15.7-2 9.5) ±0.5℃, the critical temperature for discoloration from purple to green is (22.6-49.8) ±0.5℃, and the critical temperature for discoloration from green to colorless is (31-60) ±0.5℃; the flashover voltage of the insulating material when the electrode spacing is 10mm is 18-21kV; the color of the top layer with high surface flashover strength is colorless; the thickness of the thermochromic layer is 0.1-0.4mm; the thickness of the top layer with high surface flashover strength is 0.02-0.1mm; the top layer with high surface flashover strength is prepared from organic polymer, curing agent, accelerator and inorganic nanoparticles.
[0023] Furthermore, the matrix is one or more of epoxy resin substrate, silicone rubber, nylon, polymethyl methacrylate, insulating paper, ceramic, glass, and epoxy resin / mica composite material.
[0024] Furthermore, the epoxy resin / mica composite material is prepared by impregnating epoxy resin into mica tape and heating and curing the mica tape.
[0025] Furthermore, the critical color change temperature of the insulating material varies with the mass ratio of cholesterol oleyl carbonate, cholesterol nonanoate, and cholesterol chloride in the thermochromic layer, specifically: When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 18:1:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10.2-31) ± 0.5 ° C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 10.2 ± 0.5 ° C, the critical color change temperature from blue to purple is 15.7 ± 0.5 ° C, the critical color change temperature from purple to green is 22.6 ± 0.5 ° C, and the critical color change temperature from green to colorless is 31 ± 0.5 ° C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 17:2:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10.3-33) ± 0.5 ° C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 10.3 ± 0.5 ° C, the critical color change temperature from blue to purple is 16 ± 0.5 ° C, the critical color change temperature from purple to green is 24.2 ± 0.5 ° C, and the critical color change temperature from green to colorless is 33 ± 0.5 ° C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 16:3:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10.3-37) ± 0.5 ° C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 10.3 ± 0.5 ° C, the critical color change temperature from blue to purple is 16.4 ± 0.5 ° C, the critical color change temperature from purple to green is 26.8 ± 0.5 ° C, and the critical color change temperature from green to colorless is 37 ± 0.5 ° C. When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 15:4:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10.4-40) ± 0.5 ° C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 10.4 ± 0.5 ° C, the critical color change temperature from blue to purple is 16.9 ± 0.5 ° C, the critical color change temperature from purple to green is 28.3 ± 0.5 ° C, and the critical color change temperature from green to colorless is 40 ± 0.5 ° C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 14:5:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10.6-43) ± 0.5 ° C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 10.6 ± 0.5 ° C, the critical color change temperature from blue to purple is 17.4 ± 0.5 ° C, the critical color change temperature from purple to green is 30.1 ± 0.5 ° C, and the critical color change temperature from green to colorless is 43 ± 0.5 ° C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 13:6:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10.9-46) ± 0.5 ° C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 10.9 ± 0.5 ° C, the critical color change temperature from blue to purple is 17.8 ± 0.5 ° C, the critical color change temperature from purple to green is 32.2 ± 0.5 ° C, and the critical color change temperature from green to colorless is 46 ± 0.5 ° C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 12:7:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (11.2-50)±0.5°C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 11.2±0.5°C, the critical color change temperature from blue to purple is 18.6±0.5°C, the critical color change temperature from purple to green is 35.4±0.5°C, and the critical color change temperature from green to colorless is 50±0.5°C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 11:8:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (11.8-53)±0.5°C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 11.8±0.5°C, the critical color change temperature from blue to purple is 19.5±0.5°C, the critical color change temperature from purple to green is 37.5±0.5°C, and the critical color change temperature from green to colorless is 53±0.5°C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 10:9:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (12.2-55.1)±0.5°C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 12.2±0.5°C, the critical color change temperature from blue to purple is 20.4±0.5°C, the critical color change temperature from purple to green is 40.5±0.5°C, and the critical color change temperature from green to colorless is 55.1±0.5°C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 9:10:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (13.4-56.1)±0.5°C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 13.4±0.5°C, the critical color change temperature from blue to purple is 22.1±0.5°C, the critical color change temperature from purple to green is 42.6±0.5°C, and the critical color change temperature from green to colorless is 56.1±0.5°C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 8:11:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (15.5-57.6)±0.5°C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 15.5±0.5°C, the critical color change temperature from blue to purple is 24.4±0.5°C, the critical color change temperature from purple to green is 45.2±0.5°C, and the critical color change temperature from green to colorless is 57.6±0.5°C; When the mass ratio of the cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 7:12:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (18.1-58.3)±0.5°C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 18.1±0.5°C, the critical color change temperature from blue to purple is 27.3±0.5°C, the critical color change temperature from purple to green is 47.7±0.5°C, and the critical color change temperature from green to colorless is 58.3±0.5°C; When the mass ratio of cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is 6:13:1, the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (20-60)±0.5℃; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 20±0.5℃, the critical color change temperature from blue to purple is 29.5±0.5℃, the critical color change temperature from purple to green is 49.8±0.5℃, and the critical color change temperature from green to colorless is 60±0.5℃.
[0026] Furthermore, the organic polymer is an epoxy resin prepolymer, and its epoxy value is 0.4-0.6eq / 100g, epoxy equivalent is 170-190g / ep, viscosity is 10000-15000mPa•s, and chromaticity is 0.1.
[0027] Furthermore, the curing agent is methyltetrahydrophthalic anhydride.
[0028] Furthermore, the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol.
[0029] Furthermore, the inorganic nanoparticles are aluminum oxide (Al 2 O 3 ), the particle size of inorganic nanoparticles is ≤100nm.
[0030] The present invention also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of the power equipment, select a matrix for simulation according to the Poisson equation, the current continuity equation and the solid heat transfer equation, set simulation parameters, and obtain the temperature change range of the matrix through temperature change and flow coupling calculation in the model; Step 2, heating and stirring cholesterol oleyl carbonate, cholesterol nonanoate, cholesterol chloride and alkanol together in an oil bath to obtain a liquid crystal mixture; Step 3, grinding the substrate surface with grinding paper and then wiping it with alcohol, and evenly spin-coating the liquid crystal mixture on the wiped substrate surface to obtain a thermochromic layer; Step 4: at room temperature, dissolving the organic polymer, curing agent and accelerator in an organic solvent by stirring to obtain a uniform organic phase solution, then adding the inorganic nanoparticles and continuing to stir, and after the stirring is completed, ultrasonically obtaining a suspension; Step 5: spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, and then put it into a drying oven to solidify at normal pressure to obtain the insulating material.
[0031] Furthermore, the model in step 1 is set to alternating current, with a sinusoidal period of 100us, a simulation time of 200us, and a step length of 5us.
[0032] Furthermore, in the setting of the model parameters in step 1, the dielectric constant (ε) of the matrix is 2-5, the conductivity ( ) is 1×10 -16 -1×10 -14 S / m, thermal conductivity is 0.1-0.5W / (m•K).
[0033] Furthermore, the calculation method in step 1 is one or more of the backward difference formula (BDF) method, the generalized α method, the explicit Runge-Kutta method or the Adams-Bashforth method for solving ordinary differential equations (ODE).
[0034] Furthermore, the matrix in step 1 is one or more of epoxy resin substrate, silicone rubber, nylon, polymethyl methacrylate, insulating paper, ceramic, glass, epoxy resin / mica composite material.
[0035] Furthermore, the epoxy resin / mica composite material is prepared by impregnating epoxy resin into mica tape and heating and curing the mica tape.
[0036] Furthermore, in step 1, the temperature of the substrate varies in the range of 0-60°C.
[0037] Furthermore, in the step 2, the mass ratio of the total mass of cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride to the alkanol is (1:1)-(2:1).
[0038] Furthermore, in step 2, the mass ratio of cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride is (6-18):(1-13):1.
[0039] Furthermore, the alkanol in step 2 is one or more of hexadecanol, nonadecanol, heneicosanol, hexacosanol, heptacosanol, octacosanol and triacontanol.
[0040] Furthermore, the heating and stirring temperature in step 2 is 96-110° C., the heating and stirring speed is 800-1000 r / min, and the heating and stirring time is 1-2 h.
[0041] Furthermore, in step 3, the rotation speed of the spin coating is 300-1200 r / min, and the spin coating time is 10-50 s.
[0042] Furthermore, the particle size of the grinding paper in step 3 is 800-1200 Cw.
[0043] Furthermore, in step 3, the temperature range in which the thermochromic layer changes from blue to purple, then from purple to green, and then from green to colorless is (10-60) ± 0.5°C; The critical color change temperatures of the thermochromic layer are as follows: the critical color change temperature from colorless to blue is (10.2-20)±0.5°C, the critical color change temperature from blue to purple is (15.7-29.5)±0.5°C, the critical color change temperature from purple to green is (22.6-49.8)±0.5°C, and the critical color change temperature from green to colorless is (31-60)±0.5°C.
[0044] Furthermore, in the step 3, the temperature variation range of the substrate is consistent with the temperature variation range of the thermochromic layer.
[0045] Furthermore, in step 3, the thickness of the thermochromic layer is 0.1-0.4 mm.
[0046] Furthermore, the color changing principle of the cholesteric liquid crystal in the thermochromic layer in step 3 is that the cholesteric liquid crystal has a spiral molecular orientation arrangement structure, and under the illumination of white light, it will reflect different colors; when the temperature changes, the pitch of the cholesteric liquid crystal is caused P The change in temperature causes the wavelength of the Bragg reflected light to change, so the cholesteric liquid crystal produces a thermochromic effect under temperature changes.
[0047] Furthermore, the cholesteric liquid crystal in the thermochromic layer in step 3 has poor compatibility with the matrix. When the cholesteric liquid crystal is mixed with the matrix alone, the spiral structure of the cholesteric liquid crystal will be destroyed and the thermochromic property cannot be achieved. However, the alkanol has good compatibility with the cholesteric liquid crystal, so that the cholesteric liquid crystal maintains an excellent color-changing effect. At the same time, the alkanol has a large adhesive force. After mixing with the cholesteric liquid crystal, the thermochromic layer can be better bonded to the matrix, and the mixing with the cholesteric liquid crystal will not affect its color-changing performance.
[0048] Furthermore, in step 4, the mass ratio of the organic polymer, the curing agent and the accelerator is (80-120): (50-100): 1.
[0049] Furthermore, in step 4, the mass-to-volume ratio of the organic polymer to the organic solvent is 3:20, wherein the unit of mass is g and the unit of volume is mL.
[0050] Furthermore, the amount of the inorganic nanoparticles added in step 4 is 1-5% of the total mass of the top layer with high surface flashover strength.
[0051] Furthermore, the organic polymer in step 4 is an epoxy resin prepolymer, and its epoxy value is 0.4-0.6eq / 100g, epoxy equivalent is 170-190g / ep, viscosity is 10000-15000mPa•s, and chromaticity is 0.1.
[0052] Furthermore, the curing agent in step 4 is methyltetrahydrophthalic anhydride.
[0053] Furthermore, the promoter in step 4 is 2,4,6-tris(dimethylaminomethyl)phenol.
[0054] Furthermore, the organic solvent in step 4 is ethyl acetate.
[0055] Furthermore, the stirring and dissolving speed in step 4 is 300-800 r / min, and the stirring time is 10-20 min.
[0056] Furthermore, the inorganic nanoparticles in step 4 are aluminum oxide (Al 2 O 3 ), the particle size of inorganic nanoparticles is ≤100nm.
[0057] Furthermore, in step 4, the speed of continued stirring is 300-800 r / min, and the time of continued stirring is 5-20 min.
[0058] Furthermore, the frequency of the ultrasound in step 4 is 20-50kHz, and the time of the ultrasound is 10-30min.
[0059] Furthermore, the inorganic nanoparticles in the suspension in step 4 will introduce shallow charge traps, accelerate surface charge dissipation, and suppress the electric field distortion problem caused by surface charge accumulation, thereby improving the surface flashover intensity.
[0060] Furthermore, in step 5, the pressure of the spray gun is 20-50 psi, the distance between the spray gun and the thermochromic layer is 100-200 mm, the spraying angle between the spray gun and the thermochromic layer is 45-120°, the needle size of the spray gun is 0.1-0.5 mm, and the flow rate of the spray gun is 5-20 mL / min.
[0061] Furthermore, the spraying time in step 5 is 30-90s.
[0062] Furthermore, in step 5, the curing temperature is 60-120° C., and the curing time is 5-10 hours.
[0063] Furthermore, the thickness of the top layer with high surface flashover strength in step 5 is 0.02-0.1 mm.
[0064] Furthermore, when the suspension in step 5 is sprayed on the thermochromic layer, the hydroxyl groups in the alkanol can open the ring of the epoxy resin in the suspension, and the two react chemically to form a cross-linked polyether structure, so that the thermochromic layer and the top layer with high surface flashover strength form a stable chemical connection.
[0065] Furthermore, the insulating material is used to detect abnormal heat accumulation caused by insulation structure defects in power equipment.
[0066] Beneficial Effects of the Invention 1. Traditional thermochromic materials can only achieve changes in the depth of a single color, while the present invention uses cholesteric liquid crystal materials, so that the material can display different color changes with different temperature changes, and avoids the cumbersome process of preparing cholesteric liquid crystals into microcapsules and then mixing them with a matrix; the thermochromic layer in the present invention is prepared by mixing cholesteric liquid crystals and alkanols, and the alkanols act as anchoring agents in the thermochromic layer, which provide adhesion to fix the thermochromic layer on the matrix, and the anchoring agent material does not affect the color development of the cholesteric liquid crystals. The finally obtained cholesteric liquid crystals can achieve multi-color color changes with temperature, and the color can be used to more accurately characterize the temperature change. In addition, the thickness range of the thermochromic layer in the present invention is moderate, avoiding the problems of slow heat transfer and uneven heat transfer caused by too thick a thermochromic layer, and also avoiding the problem of uneven color development caused by too thin a thermochromic layer. In addition, the appropriate ratio of cholesteric liquid crystals to alkanols prevents the alkanols from affecting the color change effect of the thermochromic layer due to excessive addition, and affects the bonding effect due to too low an addition; 2. The present invention uses alkanol for mixing in the thermochromic layer. This is different from the thermosetting material, which produces a chemical reaction and cross-linking after reaching the curing temperature due to the temperature rise during the curing process after mixing with the cholesteric liquid crystal. After curing, chemical bonds are generated between molecules to form a three-dimensional network structure. The chains cannot slide between each other, and the cholesteric liquid crystal cannot produce a change in pitch and change color in it. It is also different from other thermoplastic resins that have poor compatibility with cholesteric liquid crystals, resulting in uneven dispersion and poor color development during mixing with cholesteric liquid crystals. The molecular structures of the alkanol and cholesteric liquid crystal in the present invention are relatively similar and have good compatibility. Therefore, after mixing the cholesteric liquid crystal with the alkanol, a thermochromic layer that changes with the mass ratio of cholesterol oleyl carbonate, cholesterol nonanoate, and cholesterol chloride in the cholesteric liquid crystal is obtained, and a layer with unique color change conditions is obtained; 3. The insulating material in the present invention is a double-layer structure, including a matrix, a thermochromic layer and a high surface flashover strength top layer, wherein the thermochromic layer is composed of a mixture of cholesteric liquid crystal and alkanol, and the high surface flashover strength top layer is composed of a mixture of organic polymer, curing agent, accelerator and inorganic nanoparticles. The thermochromic layer can change different colors as the temperature of the system increases, thereby judging the temperature of the system, and the high surface flashover strength top layer can regulate surface properties such as trap distribution and conductivity, and inhibit surface charge accumulation. At the same time, the insulating material also has high mechanical strength, wear resistance and other properties, and is suitable for internal insulation and outdoor insulation of power equipment. Even under the effects of high humidity, rain, dirt layer and mechanical stress outdoors, it can still work stably; 4. The top layer of the present invention with high surface flashover strength is made of thermosetting materials such as epoxy resin prepolymer with high mechanical properties, and Al is doped in the epoxy resin prepolymer. 2 O 3 Nanofillers can effectively regulate the distribution of surface traps and improve the flashover strength along the surface, and a small amount of Al is doped 2 O 3 The mechanical strength of the coating will not be reduced, and the insulating material prepared in this way can maintain good strength when simulating ordinary precipitation erosion and strong winds, and the top layer with high surface flashover strength is colorless and will not affect the color change of the thermochromic layer below; 5. The insulating material of the present invention can intuitively and in real time display the surface temperature change of the insulating structure, and at the same time improve the flashover strength along the insulation surface. The preparation process is simple, the spraying application is convenient, and it is suitable for large-scale production applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 is a schematic diagram of the layer structure of the insulating material described in the present invention; Figure 2 This is a color change diagram of the insulating material described in Example 14 at 0-55°C; Figure 3 A comparison diagram of the flashover voltage of the insulating materials in Examples 14-18 of the present invention and Comparative Examples 1-2; Figure 4 Surface trap distribution diagrams of the insulating materials described in Examples 14-17 and the insulating materials in Comparative Examples 1-2; Figure 5 is a scanning electron microscope (SEM) image of a cross section of the insulating material described in Example 14; Figure 6 This is a surface scanning electron microscope (SEM) image of the insulating material described in Example 14; Figure 7 This is a graph showing the results of testing the insulating material described in Example 14 50 times using the tape stripping method. DETAILED DESCRIPTION
[0068] The invention is described in detail below with reference to the embodiments: The present invention prepares a thermochromic layer by mixing cholesteric liquid crystal and alkanol, so that the insulating material can present different colors with different temperature changes, and mixes organic polymers and inorganic nanoparticles to prepare a top layer with high surface flashover strength, so that the top layer with high surface flashover strength can regulate surface properties such as trap distribution and conductivity, and inhibit surface charge accumulation.
[0069] Example 1 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10.2-31) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 18:1:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0070] The critical color change temperatures of the thermochromic layer described in this embodiment are: the critical color change temperature from colorless to blue is 10.2±0.5℃, the critical color change temperature from blue to purple is 15.7±0.5℃, the critical color change temperature from purple to green is 22.6±0.5℃, and the critical color change temperature from green to colorless is 31±0.5℃.
[0071] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: 1.98 g of cholesterol oleyl carbonate, 0.11 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol were heated and stirred in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and the liquid crystal mixture was applied at a rotation speed of 500 r / min for 15 s to form a film, and cured at 80°C for 8 h to obtain the thermochromic layer.
[0072] Example 2 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.14 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10.3-33) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 17:2:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0073] The critical color change temperatures of the thermochromic layer described in this embodiment are: the critical color change temperature from colorless to blue is 10.3±0.5℃, the critical color change temperature from blue to purple is 16±0.5℃, the critical color change temperature from purple to green is 24.2±0.5℃, and the critical color change temperature from green to colorless is 33±0.5℃.
[0074] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.87 g of cholesterol oleyl carbonate, 0.22 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0075] Example 3 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10.3-37) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 16:3:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0076] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 10.3±0.5℃, the critical color change temperature from blue to purple is 16.4±0.5℃, the critical color change temperature from purple to green is 26.8±0.5℃, and the critical color change temperature from green to colorless is 37±0.5℃.
[0077] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.76 g of cholesterol oleyl carbonate, 0.33 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0078] Example 4 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.16 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10.4-40) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 15:4:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0079] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 10.4±0.5℃, the critical color change temperature from blue to purple is 16.9±0.5℃, the critical color change temperature from purple to green is 28.3±0.5℃, and the critical color change temperature from green to colorless is 40±0.5℃.
[0080] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.65 g of cholesterol oleyl carbonate, 0.44 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0081] Example 5 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10.6-43) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 14:5:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0082] The critical color change temperatures of the thermochromic layer described in this embodiment are: the critical color change temperature from colorless to blue is 10.6±0.5℃, the critical color change temperature from blue to purple is 17.4±0.5℃, the critical color change temperature from purple to green is 30.1±0.5℃, and the critical color change temperature from green to colorless is 43±0.5℃.
[0083] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.54 g of cholesterol oleyl carbonate, 0.55 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0084] Example 6 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.16 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10.9-46) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 13:6:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0085] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 10.9±0.5℃, the critical color change temperature from blue to purple is 17.8±0.5℃, the critical color change temperature from purple to green is 32.2±0.5℃, and the critical color change temperature from green to colorless is 46±0.5℃.
[0086] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.43 g of cholesterol oleyl carbonate, 0.66 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0087] Example 7 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (11.2-50)±0.5°C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 12:7:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0088] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 11.2±0.5℃, the critical color change temperature from blue to purple is 18.6±0.5℃, the critical color change temperature from purple to green is 35.4±0.5℃, and the critical color change temperature from green to colorless is 50±0.5℃.
[0089] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.32 g of cholesterol oleyl carbonate, 0.77 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0090] Example 8 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (11.8-53) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 11:8:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0091] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 11.8±0.5℃, the critical color change temperature from blue to purple is 19.5±0.5℃, the critical color change temperature from purple to green is 37.5±0.5℃, and the critical color change temperature from green to colorless is 53±0.5℃.
[0092] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.21 g of cholesterol oleyl carbonate, 0.88 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0093] Example 9 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.14 mm; the color of the thermochromic layer changes with its temperature, specifically: at (12.2-55.1)±0.5°C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 10:9:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0094] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 12.2±0.5℃, the critical color change temperature from blue to purple is 20.4±0.5℃, the critical color change temperature from purple to green is 40.5±0.5℃, and the critical color change temperature from green to colorless is 55.1±0.5℃.
[0095] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0096] Example 10 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (13.4-56.1) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 9:10:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0097] The critical color change temperatures of the thermochromic layer described in this embodiment are: the critical color change temperature from colorless to blue is 13.4±0.5℃, the critical color change temperature from blue to purple is 22.1±0.5℃, the critical color change temperature from purple to green is 42.6±0.5℃, and the critical color change temperature from green to colorless is 56.1±0.5℃.
[0098] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 0.99 g of cholesterol oleyl carbonate, 1.1 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture. Apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0099] Embodiment 11 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (15.5-57.6) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 8:11:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0100] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 15.5±0.5℃, the critical color change temperature from blue to purple is 24.4±0.5℃, the critical color change temperature from purple to green is 45.2±0.5℃, and the critical color change temperature from green to colorless is 57.6±0.5℃.
[0101] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 0.88 g of cholesterol oleyl carbonate, 1.21 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0102] Example 12 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.16 mm; the color of the thermochromic layer changes with its temperature, specifically: at (18.1-58.3)±0.5°C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 7:12:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0103] The critical color change temperatures of the thermochromic layer in this embodiment are: the critical color change temperature from colorless to blue is 18.1±0.5℃, the critical color change temperature from blue to purple is 27.3±0.5℃, the critical color change temperature from purple to green is 47.7±0.5℃, and the critical color change temperature from green to colorless is 58.3±0.5℃.
[0104] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 0.77 g of cholesterol oleyl carbonate, 1.32 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 500 r / min for 15 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0105] Example 13 The present embodiment provides a thermochromic layer, which is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.15 mm; the color of the thermochromic layer changes with its temperature, specifically: at (20-60) ± 0.5 ° C, the color changes to colorless, blue, purple, green and colorless in sequence; the cholesteric liquid crystal includes cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC) in a mass ratio of 6:13:1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate (COC), cholesterol nonanoate (CEP) and cholesterol chloride (CC).
[0106] The critical color change temperatures of the thermochromic layer described in this embodiment are: the critical color change temperature from colorless to blue is 20±0.5℃, the critical color change temperature from blue to purple is 29.5±0.5℃, the critical color change temperature from purple to green is 49.8±0.5℃, and the critical color change temperature from green to colorless is 60±0.5℃.
[0107] This embodiment also provides a method for preparing the thermochromic layer, comprising the following steps: Step 1. Heat and stir 0.66 g of cholesterol oleyl carbonate, 1.43 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of alkanol in an oil bath at 96°C for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture, and apply the liquid crystal mixture at a rotation speed of 1000 r / min for 30 seconds to form a film, and cure it at 80°C for 8 hours to obtain the thermochromic layer.
[0108] Embodiment 14 The present embodiment provides an insulating material including a thermochromic layer, wherein the insulating material is prepared from bottom to top in sequence from a matrix, the thermochromic layer and a top layer with high surface flashover strength; the color of the insulating material changes with its temperature, specifically: the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (12.2-55.1)±0.5℃; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 12.2±0.5℃, the critical color change temperature from blue to purple is 12.2±0.5℃, and the critical color change temperature from blue to purple is 12.2±0.5℃. The critical temperature is 20.4±0.5℃, the critical temperature for discoloration from purple to green is 40.5±0.5℃, and the critical temperature for discoloration from green to colorless is 55.1±0.5℃; the flashover voltage of the insulating material is 18.8kV when the electrode spacing is 10mm; the color of the top layer with high surface flashover strength is colorless; the thickness of the thermochromic layer is 0.15mm; the thickness of the top layer with high surface flashover strength is 0.05mm; the top layer with high surface flashover strength is prepared from organic polymer, curing agent, accelerator and inorganic nanoparticles.
[0109] This embodiment also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of power equipment. According to Poisson's equation, current continuity equation and solid heat transfer equation, select epoxy resin substrate as the matrix for simulation. In the model, set alternating current, its sine period is 100us, simulation time is 200us, and step length is 5us; in the model, set the dielectric constant (ε) of epoxy resin to 4, and the conductivity ( ) is 3.067×10 -15 S / m, thermal conductivity is 0.2W / (m•K); through the temperature change and flow coupling in the model, the backward difference formula (BDF) method is used to calculate that the temperature change range of the matrix is 12-56.18℃; Step 2, 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of triacontanol were heated and stirred in an oil bath at 96° C. for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture; Step 3, polishing the surface of the epoxy resin substrate with 1200Cw grinding paper and then wiping it with alcohol, and applying the liquid crystal mixed solution to the wiped surface of the epoxy resin substrate at a rotation speed of 500r / min for 15s to obtain a thermochromic layer; Step 4: at room temperature, 3 g of epoxy resin prepolymer, 2.4 g of methyltetrahydrophthalic anhydride and 0.03 g of 2,4,6-tris(dimethylaminomethyl)phenol were dissolved in 20 mL of ethyl acetate under stirring at 800 r / min for 10 min to obtain a uniform organic phase solution, and then 0.06 g of aluminum oxide was added and continued to stir for 10 min. After the stirring was completed, ultrasonic treatment was performed at 40 kHz for 20 min to obtain a suspension; Step 5: Spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, wherein the pressure of the spray gun is 40 psi, the distance between the spray gun and the thermochromic layer is 150 mm, the spraying angle between the spray gun and the thermochromic layer is 90°, the needle size of the spray gun is 0.3 mm, the flow rate of the spray gun is 10 mL / min, and the spraying time is 60 s. After spraying, the material is placed in a vacuum box and cured at 80° C. and normal pressure for 8 hours to obtain the insulating material.
[0110] The epoxy value of the epoxy resin prepolymer in this embodiment is 0.537eq / 100g (epoxy equivalent is 186.2g / ep), the viscosity is 12460mPa•s, and the chromaticity is 0.1; the aluminum oxide (Al 2 O 3 ) has a particle size of 30±5nm.
[0111] Embodiment 15 The present embodiment provides an insulating material including a thermochromic layer, wherein the insulating material is prepared from bottom to top in sequence from a matrix, the thermochromic layer and a top layer with high surface flashover strength; the color of the insulating material changes with its temperature, specifically: the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (12.2-55.1)±0.5℃; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 12.2±0.5℃, the critical color change temperature from blue to purple is 12.2±0.5℃, and the critical color change temperature from blue to purple is 12.2±0.5℃. The critical temperature is 20.4±0.5℃, the critical temperature for discoloration from purple to green is 40.5±0.5℃, and the critical temperature for discoloration from green to colorless is 55.1±0.5℃; the flashover voltage of the insulating material is 19.5kV when the electrode spacing is 10mm; the color of the top layer with high surface flashover strength is colorless; the thickness of the thermochromic layer is 0.15mm; the thickness of the top layer with high surface flashover strength is 0.05mm; the top layer with high surface flashover strength is prepared from organic polymer, curing agent, accelerator and inorganic nanoparticles.
[0112] This embodiment also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of power equipment. According to Poisson's equation, current continuity equation and solid heat transfer equation, select epoxy resin substrate as the matrix for simulation. In the model, set alternating current, its sine period is 100us, simulation time is 200us, and step length is 5us; in the model, set the dielectric constant (ε) of epoxy resin to 4, and the conductivity ( ) is 3.067×10 -15 S / m, thermal conductivity is 0.2W / (m•K); through the temperature change and flow coupling in the model, the backward difference formula (BDF) method is used to calculate that the temperature change range of the matrix is 12-53.46℃; Step 2, 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of triacontanol were heated and stirred in an oil bath at 96° C. for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture; Step 3, polishing the surface of the epoxy resin substrate with 1200Cw grinding paper and then wiping it with alcohol, and applying the liquid crystal mixed solution to the wiped surface of the epoxy resin substrate at a rotation speed of 500r / min for 15s to obtain a thermochromic layer; Step 4: at room temperature, 3 g of epoxy resin prepolymer, 2.4 g of methyltetrahydrophthalic anhydride and 0.03 g of 2,4,6-tris(dimethylaminomethyl)phenol were dissolved in 20 mL of ethyl acetate under stirring at 800 r / min for 10 min to obtain a uniform organic phase solution, and then 0.17 g of aluminum oxide was added and continued to stir for 10 min. After the stirring was completed, ultrasonic treatment was performed at 40 kHz for 20 min to obtain a suspension; Step 5: Spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, wherein the pressure of the spray gun is 40 psi, the distance between the spray gun and the thermochromic layer is 150 mm, the spraying angle between the spray gun and the thermochromic layer is 90°, the needle size of the spray gun is 0.3 mm, the flow rate of the spray gun is 10 mL / min, and the spraying time is 60 s. After spraying, the material is placed in a vacuum box and cured at 80° C. and normal pressure for 8 hours to obtain the insulating material.
[0113] The epoxy value of the epoxy resin prepolymer in this embodiment is 0.537eq / 100g (epoxy equivalent is 186.2g / ep), the viscosity is 12460mPa•s, and the chromaticity is 0.1; the aluminum oxide (Al 2 O 3 ) has a particle size of 30±5nm.
[0114] Example 16 The present embodiment provides an insulating material including a thermochromic layer, wherein the insulating material is prepared from bottom to top in sequence from a matrix, the thermochromic layer and a top layer with high surface flashover strength; the color of the insulating material changes with its temperature, specifically: the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (12.2-55.1)±0.5℃; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 12.2±0.5℃, the critical color change temperature from blue to purple is 12.2±0.5℃, and the critical color change temperature from blue to purple is 12.2±0.5℃. The critical temperature is 20.4±0.5℃, the critical temperature of discoloration from purple to green is 40.5±0.5℃, and the critical temperature of discoloration from green to colorless is 55.1±0.5℃; the flashover voltage of the insulating material is 19.6kV when the electrode spacing is 10mm; the color of the top layer with high surface flashover strength is colorless; the thickness of the thermochromic layer is 0.15mm; the thickness of the top layer with high surface flashover strength is 0.05mm; the top layer with high surface flashover strength is prepared from organic polymer, curing agent, accelerator and inorganic nanoparticles.
[0115] This embodiment also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of power equipment. According to Poisson's equation, current continuity equation and solid heat transfer equation, select epoxy resin substrate as the matrix for simulation. In the model, set alternating current, its sine period is 100us, simulation time is 200us, and step length is 5us; in the model, set the dielectric constant (ε) of epoxy resin to 4, and the conductivity ( ) is 3.067×10 -15 S / m, thermal conductivity is 0.2W / (m•K); through the temperature change and flow coupling in the model, the backward difference formula (BDF) method is used to calculate that the temperature change range of the matrix is 12-56.18℃; Step 2, 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of triacontanol were heated and stirred in an oil bath at 96° C. for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture; Step 3, polishing the surface of the epoxy resin substrate with 1200Cw grinding paper and then wiping it with alcohol, and applying the liquid crystal mixed solution to the wiped surface of the epoxy resin substrate at a rotation speed of 500r / min for 15s to obtain a thermochromic layer; Step 4: at room temperature, 3 g of epoxy resin prepolymer, 2.4 g of methyltetrahydrophthalic anhydride and 0.03 g of 2,4,6-tris(dimethylaminomethyl)phenol were dissolved in 20 mL of ethyl acetate under stirring at 800 r / min for 10 min to obtain a uniform organic phase solution, and then 0.23 g of aluminum oxide was added and continued to stir for 10 min. After the stirring was completed, ultrasonic treatment was performed at 40 kHz for 20 min to obtain a suspension; Step 5: Spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, wherein the pressure of the spray gun is 40 psi, the distance between the spray gun and the thermochromic layer is 150 mm, the spraying angle between the spray gun and the thermochromic layer is 90°, the needle size of the spray gun is 0.3 mm, the flow rate of the spray gun is 10 mL / min, and the spraying time is 60 s. After spraying, the material is placed in a vacuum box and cured at 80° C. and normal pressure for 8 hours to obtain the insulating material.
[0116] The epoxy value of the epoxy resin prepolymer in this embodiment is 0.537eq / 100g (epoxy equivalent is 186.2g / ep), the viscosity is 12460mPa•s, and the chromaticity is 0.1; the aluminum oxide (Al 2 O 3 ) has a particle size of 30±5nm.
[0117] Embodiment 17 The present embodiment provides an insulating material including a thermochromic layer, wherein the insulating material is prepared from bottom to top in sequence from a matrix, the thermochromic layer and a top layer with high surface flashover strength; the color of the insulating material changes with its temperature, specifically: the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (12.2-55.1)±0.5℃; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 12.2±0.5℃, the critical color change temperature from blue to purple is 12.2±0.5℃, and the critical color change temperature from blue to purple is 12.2±0.5℃. The critical temperature is 20.4±0.5℃, the critical temperature for discoloration from purple to green is 40.5±0.5℃, and the critical temperature for discoloration from green to colorless is 55.1±0.5℃; the flashover voltage of the insulating material is 20.2kV when the electrode spacing is 10mm; the color of the top layer with high surface flashover strength is colorless; the thickness of the thermochromic layer is 0.15mm; the thickness of the top layer with high surface flashover strength is 0.05mm; the top layer with high surface flashover strength is prepared from organic polymer, curing agent, accelerator and inorganic nanoparticles.
[0118] This embodiment also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of power equipment. According to Poisson's equation, current continuity equation and solid heat transfer equation, select epoxy resin substrate as the matrix for simulation. In the model, set alternating current, its sine period is 100us, simulation time is 200us, and step length is 5us; in the model, set the dielectric constant (ε) of epoxy resin to 4, and the conductivity ( ) is 3.067×10 -15 S / m, thermal conductivity is 0.2W / (m•K); through the temperature change and flow coupling in the model, the backward difference formula (BDF) method is used to calculate that the temperature change range of the matrix is 12-56.18℃; Step 2, 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of triacontanol were heated and stirred in an oil bath at 96° C. for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture; Step 3, polishing the surface of the epoxy resin substrate with 1200Cw grinding paper and then wiping it with alcohol, and applying the liquid crystal mixed solution to the wiped surface of the epoxy resin substrate at a rotation speed of 500r / min for 15s to obtain a thermochromic layer; Step 4: at room temperature, 3 g of epoxy resin prepolymer, 2.4 g of methyltetrahydrophthalic anhydride and 0.03 g of 2,4,6-tris(dimethylaminomethyl)phenol were dissolved in 20 mL of ethyl acetate under stirring at 800 r / min for 10 min to obtain a uniform organic phase solution, and then 0.29 g of aluminum oxide was added and stirring was continued for 10 min. After stirring, ultrasonication was performed at 40 kHz for 20 min to obtain a suspension; Step 5: Spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, wherein the pressure of the spray gun is 40 psi, the distance between the spray gun and the thermochromic layer is 150 mm, the spraying angle between the spray gun and the thermochromic layer is 90°, the needle size of the spray gun is 0.3 mm, the flow rate of the spray gun is 10 mL / min, and the spraying time is 60 s. After spraying, the material is placed in a vacuum box and cured at 80° C. and normal pressure for 8 hours to obtain the insulating material.
[0119] The epoxy value of the epoxy resin prepolymer in this embodiment is 0.537eq / 100g (epoxy equivalent is 186.2g / ep), the viscosity is 12460mPa•s, and the chromaticity is 0.1; the aluminum oxide (Al 2 O 3 ) has a particle size of 30±5nm.
[0120] Embodiment 18 The present embodiment provides an insulating material including a thermochromic layer, wherein the insulating material is prepared from bottom to top in sequence from a matrix, the thermochromic layer and a top layer with high surface flashover strength; the color of the insulating material changes with its temperature, specifically: the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (12.2-55.1)±0.5℃; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is 12.2±0.5℃, the critical color change temperature from blue to purple is 12.2±0.5℃, and the critical color change temperature from blue to purple is 12.2±0.5℃. The critical temperature is 20.4±0.5℃, the critical temperature of discoloration from purple to green is 40.5±0.5℃, and the critical temperature of discoloration from green to colorless is 55.1±0.5℃; the flashover voltage of the insulating material is 20.3kV when the electrode spacing is 10mm; the color of the top layer with high surface flashover strength is colorless; the thickness of the thermochromic layer is 0.15mm; the thickness of the top layer with high surface flashover strength is 0.05mm; the top layer with high surface flashover strength is prepared from organic polymer, curing agent, accelerator and inorganic nanoparticles.
[0121] This embodiment also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of power equipment. According to Poisson's equation, current continuity equation and solid heat transfer equation, select epoxy resin substrate as the matrix for simulation. In the model, set alternating current, its sine period is 100us, simulation time is 200us, and step length is 5us; in the model, set the dielectric constant (ε) of epoxy resin to 4, and the conductivity ( ) is 3.067×10 -15 S / m, thermal conductivity is 0.2W / (m•K); through the temperature change and flow coupling in the model, the backward difference formula (BDF) method is used to calculate that the temperature change range of the matrix is 12-56.18℃; Step 2, 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of triacontanol were heated and stirred in an oil bath at 96° C. for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture; Step 3, polishing the surface of the epoxy resin substrate with 1200Cw grinding paper and then wiping it with alcohol, and applying the liquid crystal mixed solution to the wiped surface of the epoxy resin substrate at a rotation speed of 500r / min for 15s to obtain a thermochromic layer; Step 4: at room temperature, 3 g of epoxy resin prepolymer, 2.4 g of methyltetrahydrophthalic anhydride and 0.03 g of 2,4,6-tris(dimethylaminomethyl)phenol were dissolved in 20 mL of ethyl acetate under stirring at 800 r / min for 10 min to obtain a uniform organic phase solution, and then 0.29 g of aluminum oxide was added and stirring was continued for 10 min. After stirring, ultrasonication was performed at 40 kHz for 20 min to obtain a suspension; Step 5: Spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, wherein the pressure of the spray gun is 40 psi, the distance between the spray gun and the thermochromic layer is 150 mm, the spraying angle between the spray gun and the thermochromic layer is 90°, the needle size of the spray gun is 0.3 mm, the flow rate of the spray gun is 10 mL / min, and the spraying time is 60 s. After spraying, the material is placed in a vacuum box and cured at 80° C. and normal pressure for 8 hours to obtain the insulating material.
[0122] The epoxy value of the epoxy resin prepolymer in this embodiment is 0.537eq / 100g (epoxy equivalent is 186.2g / ep), the viscosity is 12460mPa•s, and the chromaticity is 0.1; the aluminum oxide (Al 2 O 3 ) has a particle size of 30±5nm.
[0123] Comparative Example 1 This comparative example provides an insulating material, which includes a matrix, a thermochromic layer and an organic polymer top layer; the temperature change range of the insulating material is 0-60°C, and the color changes from 0-60°C are colorless, blue, purple, green, and colorless in sequence; the flashover voltage of the insulating material when the electrode spacing is 10 mm is 17.7 kV; the thermochromic layer is prepared by mixing cholesteric liquid crystal and alkanol; the organic polymer top layer is prepared by an organic polymer; and the organic polymer top layer is colorless.
[0124] This comparative example also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of power equipment. According to Poisson's equation, current continuity equation and solid heat transfer equation, select epoxy resin substrate as the matrix for simulation. In the model, set alternating current, its sine period is 100us, simulation time is 200us, and step length is 5us; in the model, set the dielectric constant (ε) of epoxy resin to 4, and the conductivity ( ) is 3.067×10 -15 S / m, thermal conductivity is 0.2W / (m•K); through the temperature change and flow coupling in the model, the backward difference formula (BDF) method is used to calculate that the temperature change range of the matrix is 12-56.18℃; Step 2, 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of triacontanol were heated and stirred in an oil bath at 96° C. for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture; Step 3, polishing the surface of the epoxy resin substrate with 1200Cw grinding paper and then wiping it with alcohol, and applying the liquid crystal mixed solution to the wiped surface of the epoxy resin substrate at a rotation speed of 500r / min for 15s to obtain a thermochromic layer; Step 4: at room temperature, 3 g of epoxy resin prepolymer, 2.4 g of methyltetrahydrophthalic anhydride and 0.03 g of 2,4,6-tris(dimethylaminomethyl)phenol were dissolved in 20 mL of ethyl acetate under stirring at 800 r / min for 10 min to obtain a uniform organic phase solution; Step 5: Spray the organic phase solution onto the thermochromic layer using a spray gun to form an organic polymer top layer, wherein the pressure of the spray gun is 40 psi, the distance between the spray gun and the thermochromic layer is 150 mm, the spray angle between the spray gun and the thermochromic layer is 90°, the needle size of the spray gun is 0.3 mm, the flow rate of the spray gun is 10 mL / min, and the spraying time is 60 s. After spraying, the material is placed in a vacuum box and cured at 80° C. and normal pressure for 8 hours to obtain the insulating material.
[0125] The epoxy value of the epoxy resin prepolymer in this comparative example is 0.537eq / 100g (epoxy equivalent is 186.2g / ep), the viscosity is 12460mPa•s, and the chromaticity is 0.1; the aluminum oxide (Al 2 O 3 ) has a particle size of 30±5nm.
[0126] Comparative Example 2 This comparative example provides an insulating material, which includes a matrix, a thermochromic layer and a top layer with high surface flashover strength; the temperature change range of the insulating material is 0-60°C, and the color changes from 0-60°C are colorless, blue, purple, green, and colorless in sequence; the flashover voltage of the insulating material when the electrode spacing is 10 mm is 19.3 kV; the thermochromic layer is prepared by mixing cholesteric liquid crystal and alkanol; the top layer with high surface flashover strength is prepared by mixing organic polymer and inorganic nanoparticles; the top layer with high surface flashover strength is colorless.
[0127] This comparative example also provides a method for preparing an insulating material, comprising the following steps: Step 1: Establish a geometric model of power equipment. According to Poisson's equation, current continuity equation and solid heat transfer equation, select epoxy resin substrate as the matrix for simulation. In the model, set alternating current, its sine period is 100us, simulation time is 200us, and step length is 5us; in the model, set the dielectric constant (ε) of epoxy resin to 4, and the conductivity ( ) is 3.067×10 -15 S / m, thermal conductivity is 0.2W / (m•K); through the temperature change and flow coupling in the model, the backward difference formula (BDF) method is used to calculate that the temperature change range of the matrix is 12-56.18℃; Step 2, 1.1 g of cholesterol oleyl carbonate, 0.99 g of cholesterol nonanoate, 0.11 g of cholesterol chloride and 2.2 g of triacontanol were heated and stirred in an oil bath at 96° C. for 1 h at a stirring speed of 800 r / min to obtain a liquid crystal mixture; Step 3, polishing the surface of the epoxy resin substrate with 1200Cw grinding paper and then wiping it with alcohol, and applying the liquid crystal mixed solution to the wiped surface of the epoxy resin substrate at a rotation speed of 500r / min for 15s to obtain a thermochromic layer; Step 4: at room temperature, 3 g of epoxy resin prepolymer, 2.4 g of methyltetrahydrophthalic anhydride and 0.03 g of 2,4,6-tris(dimethylaminomethyl)phenol were dissolved in 20 mL of ethyl acetate under stirring at 800 r / min for 10 min to obtain a uniform organic phase solution, and then 0.60 g of aluminum oxide was added and continued to stir for 10 min. After the stirring was completed, ultrasonic treatment was performed at 40 kHz for 20 min to obtain a suspension; Step 5: Spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, wherein the pressure of the spray gun is 40 psi, the distance between the spray gun and the thermochromic layer is 150 mm, the spraying angle between the spray gun and the thermochromic layer is 90°, the needle size of the spray gun is 0.3 mm, the flow rate of the spray gun is 10 mL / min, and the spraying time is 60 s. After spraying, the material is placed in a vacuum box and cured at 80° C. and normal pressure for 8 hours to obtain the insulating material.
[0128] The epoxy value of the epoxy resin prepolymer in this comparative example is 0.537eq / 100g (epoxy equivalent is 186.2g / ep), the viscosity is 12460mPa•s, and the chromaticity is 0.1; the aluminum oxide (Al 2 O 3 ) has a particle size of 30±5m.
[0129] Table 1 shows the properties of the insulating materials in Examples 14-18 and Comparative Examples 1-2 of the present invention.
[0130] As shown in Table 1, the properties of the insulating materials in Examples 14-18 and Comparative Examples 1-2 of the present invention are shown, wherein the surface flashover voltage of the insulating material without adding alumina in Comparative Example 1 is 17.7 kV, while the surface flashover voltage of the insulating material in Examples 14-18 increases with the increase of the mass percentage of alumina, and when the content of alumina in Comparative Example 2 reaches 10%, the surface flashover intensity decreases.
[0131] When no alkanol is added to the thermochromic layer of the present invention, the liquid crystal mixture has fluidity and poor adhesion and cannot be adhered to the surface of the substrate.
[0132] like Figure 1 It is a schematic diagram of the layer structure of the insulating material described in the present invention, wherein the top layer is a top layer with high surface flashover strength, the middle layer is a thermochromic layer, and the bottom layer is a matrix.
[0133] like Figure 2 This is a color change diagram of the insulating material described in Example 14 at 0-55°C, wherein the color of the insulating material is colorless at 0°C, blue at 13°C, purple at 20°C, purple at 30°C, green at 40°C, and colorless at 55°C.
[0134] like Figure 3 The figure is a comparison diagram of the flashover voltage of the insulating materials in Examples 14-18 of the present invention and Comparative Examples 1-2, wherein the surface flashover voltage of the insulating material without adding alumina in Comparative Example 1 is 17.7 kV, while the surface flashover voltage of the insulating materials described in Examples 14-18 increases with the increase of the mass percentage of alumina. When the mass percentage of alumina in Comparative Example 2 increases to 10%, the content of the added alumina is too high, resulting in the overlap of the filler interface area, thereby reducing the trap level depth of the composite coating and causing a decrease in the flashover voltage. The test conditions for the surface flashover voltage are: using a positive polarity DC voltage at 1 kVs -1 The voltage is increased at a voltage rise rate until flashover occurs, and the flashover voltage value is recorded. The two-parameter Weibull distribution is used for analysis.
[0135] like Figure 4 The surface trap distribution diagram of the insulating materials described in Examples 14-17 and the insulating materials in Comparative Examples 1-2 shows that, as the mass percentage of aluminum oxide increases, the trap energy level of the coating becomes shallower, which promotes the dissipation of surface charges, thereby improving the surface flashover strength of the insulating material; The test conditions of the surface trap distribution are as follows: the surface trap distribution of different coatings is tested by using an isothermal surface potential decay method; In the figure, the horizontal axis (Trap energy) is the trap energy level, and the vertical axis (Trap density) is the trap density.
[0136] like Figure 5 This is a scanning electron microscope (SEM) image of the cross section of the insulating material described in Example 14. It can be seen from the image that the bottom layer of the insulating material in the image is a thermochromic layer, and the top layer is a high surface flashover strength top layer, and the two coatings can be well combined.
[0137] like Figure 6 This is a surface scanning electron microscope (SEM) image of the insulating material described in Example 14. It can be seen from the image that the top surface of the high surface flashover strength has Al 2 O 3 The nanoparticles are protruding and present a micro-nano rough structure, which is beneficial to hinder the development of electron avalanche and thus increase the flashover voltage.
[0138] like Figure 7 The insulating material of Example 14 is tested 50 times by the tape stripping method. As can be seen from the figure, after the insulating material is stripped by the tape stripping method, the surface of the insulating material does not change, which indicates that the coating in the insulating material has good adhesion; The process of the tape stripping method is: the surface of the insulating material is divided into a plurality of square areas according to grid lines, and then 3M tape is pasted to the surface of the insulating material. After placing a 200g weight on the 3M tape, the 3M tape on the surface of the insulating material is stripped, and the number of stripping times is 0-50 times. During the stripping process, each square area on the surface of the insulating material is observed to see if there are defects.
[0139] The modeling and calculation process in the present invention is not limited, and ordinary technicians in the field can use existing technologies or improve them to perform simulations.
Claims
1. A thermochromic layer, characterized in that: The thermochromic layer is made of a mixture of cholesteric liquid crystal and alkanol; the thickness of the thermochromic layer is 0.1-0.4 mm; the color of the thermochromic layer changes with its temperature, specifically: at (10-60)±0.5°C, the color changes in sequence to colorless, blue, purple, green and colorless; the cholesteric liquid crystal includes cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride in a mass ratio of (6-18): (1-13): 1; the color change critical temperature of the thermochromic layer changes with the mass ratio of cholesterol oleyl carbonate, cholesterol nonanoate and cholesterol chloride.
2. The thermochromic layer according to claim 1, characterized in that: The mass ratio of the cholesteric liquid crystal to the alkanol is (1:1)-(2:1).
3. The thermochromic layer according to claim 1, characterized in that: The alkanol is one or more of hexadecanol, nonadecanol, heneicosanol, hexacosanol, heptacosanol, octacosanol and triacontanol.
4. A method for preparing the thermochromic layer according to any one of claims 1 to 3, characterized in that: The following steps are involved: Cholesterol oleyl carbonate, cholesterol nonanoate, cholesterol chloride and alkanol are heated and stirred together in an oil bath to obtain a liquid crystal mixture, and the liquid crystal mixture is spin-coated into a film and cured to obtain the thermochromic layer.
5. An insulating material comprising the thermochromic layer according to any one of claims 1 to 3, characterized in that: The insulating material is prepared from bottom to top in sequence from a matrix, the thermochromic layer and a top layer with high surface flashover strength; the color of the insulating material changes with its temperature, specifically: the temperature change range of the insulating material from blue to purple, then from purple to green, and then from green to colorless is (10-60)±0.5°C; the critical color change temperatures of the insulating material are: the critical color change temperature from colorless to blue is (10.2-20)±0.5°C, the critical color change temperature from blue to purple is (15.7-29.5)±0.5°C, and the critical color change temperature from purple to blue is (15.7-29.5)±0.5°C. The critical temperature for color change from green to colorless is (22.6-49.8)±0.5°C, and the critical temperature for color change from green to colorless is (31-60)±0.5°C; the flashover voltage of the insulating material is 18-21 kV when the electrode spacing is 10 mm; the color of the top layer with high surface flashover strength is colorless; the thickness of the thermochromic layer is 0.1-0.4 mm; the thickness of the top layer with high surface flashover strength is 0.02-0.1 mm; the top layer with high surface flashover strength is prepared from an organic polymer, a curing agent, an accelerator and inorganic nanoparticles.
6. The insulating material according to claim 5, characterized in that The inorganic nanoparticles are aluminum oxide, and the particle size of the inorganic nanoparticles is ≤100 nm.
7. A method for preparing the insulating material according to any one of claims 5 to 6, characterized in that: The following steps are involved: Step 1: Establish a geometric model of the power equipment, select a matrix for simulation according to the Poisson equation, the current continuity equation and the solid heat transfer equation, set simulation parameters, and obtain the temperature change range of the matrix through temperature change and flow coupling calculation in the model; Step 2, heating and stirring cholesterol oleyl carbonate, cholesterol nonanoate, cholesterol chloride and alkanol together in an oil bath to obtain a liquid crystal mixture; Step 3, grinding the substrate surface with grinding paper and then wiping it with alcohol, and evenly spin-coating the liquid crystal mixture on the wiped substrate surface to obtain a thermochromic layer; Step 4: at room temperature, dissolving the organic polymer, curing agent and accelerator in an organic solvent by stirring to obtain a uniform organic phase solution, then adding the inorganic nanoparticles and continuing to stir, and after the stirring is completed, ultrasonically obtaining a suspension; Step 5: spray the suspension onto the thermochromic layer using a spray gun to form a top layer with high surface flashover strength, and then put it into a drying oven to solidify at normal pressure to obtain the insulating material.
8. The preparation method according to claim 7, characterized in that: The spin coating speed in step 3 is 300-1200 r / min, and the spin coating time is 10-50 s.
9. The preparation method according to claim 7, characterized in that: The temperature variation range of the substrate in step 3 is consistent with the temperature variation range of the thermochromic layer.
10. The preparation method according to claim 7, characterized in that: The amount of the inorganic nanoparticles added in step 4 is 1-5% of the total mass of the top layer with high surface flashover strength.