Separation method of lignin-carbohydrate complex with complete structure
Through a combined system of solid-liquid extraction and biological enzymatic hydrolysis, lignocellulosic raw materials are processed under mild conditions, which solves the problems of cumbersome LCC separation methods and low yield in the existing technology, and achieves LCC separation with complete structure, which is suitable for biological applications. Applications in the field of medicine.
Patent Information
- Application Number
- CN202410968408.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
AI Technical Summary
In the existing technology, when structurally intact lignin-carbohydrate complexes (LCC) are separated from lignocellulosic raw materials, the method is cumbersome, energy-consuming, and has low yield. It is difficult to keep the connecting bonds intact, which limits the application of LCC in biomedicine. field of application.
A combined system of solid-liquid extraction and biological enzymatic hydrolysis is used to perform ball milling and enzymatic hydrolysis under mild conditions. The structural integrity of LCC is retained through steps such as Soxhlet extraction, ball milling, stirring extraction, and enzymatic hydrolysis.
It achieves process simplification, reduces energy consumption, increases productivity, and effectively retains the connection keys of LCC, making it suitable for applications in the biomedical field.
Smart Images

Figure BDA0004952391110000041 
Figure BDA0004952391110000051 
Figure BDA0004952391110000052
Abstract
Description
Technical Field
[0001] The invention relates to the field of lignocellulosic raw material extraction, and in particular to a method for separating and extracting a lignin-carbohydrate complex (LCC) with a complete structure from enzymatically hydrolyzed lignocellulosic raw materials. Background Art
[0002] Lignin-Carbohydrate Complex (LCC) is a natural polymer formed by cross-linking lignin and carbohydrates through chemical bonds. LCC is formed by combining hydrophobic rigid lignin fragments and hydrophilic flexible polysaccharide fragments, which makes it exhibit unique biological activities such as antioxidant, anti-cancer / anti-tumor, anti-viral and anti-ultraviolet, etc. It is a good medical polymer compound with considerable potential in biomedical fields such as medical care materials. Therefore, isolating a structurally complete LCC component has important basic and practical significance for the efficient utilization of LCC.
[0003] In LCC, the chemical bonds formed between lignin and polysaccharides are called lignin-carbohydrate complex linkages, including phenyl glycosidic bonds, ester bonds, and ether bonds, as well as a small amount of hemiacetal and acetal bonds. The different types and numbers of linkages in different wood fiber raw materials will cause the separated LCC to exhibit a wide range of structures and biological activities. At present, the methods commonly used to separate LCC from wood fiber raw materials are the traditional Beckmann method and the alkali extraction method. The Beckmann method is to deeply ball mill the raw materials to achieve the purpose of fiber crushing and cell wall breaking, and then extract them with solvents such as dioxane and dimethylformamide, and then use a series of solvents such as dichloroethane, ethanol and acetone to purify LCC. This method has a cumbersome process, high energy consumption and low yield; the alkali extraction method is to separate LCC from the alkaline extract. This method has a simple process, but due to the high alkalinity of the extract, the purity of the separated LCC is not high, and the linkage is not completely retained, which is not suitable for the study of the structure and mechanism of LCC. CN202310949407.8 reports a method for separating LCC using a LiCl / DMSO full-solution system-complex enzyme combination. A large amount of alkaline NaOH aqueous solution is used during the separation process, resulting in a large number of breakages of phenyl glycosidic bonds and ether bonds, causing serious damage to the LCC structure.
[0004] Therefore, the existing LCC extraction methods are cumbersome and harsh, with low yields, or difficult to separate from wood fiber raw materials in a structurally intact form, which limits the development and utilization of LCC industrial products. Summary of the invention
[0005] The present invention aims to solve the problems existing in the prior art and provides a method for separating and extracting a structurally intact lignin-carbohydrate complex (LCC) from enzymatically hydrolyzed plant fiber raw materials. The method utilizes a combined system of traditional solid-liquid extraction and biological enzymatic hydrolysis to separate and extract LCC components under mild conditions. Appropriate ball milling pretreatment helps to effectively separate the product from the wood fiber and efficiently retain the LCC connecting bonds.
[0006] In order to solve the above technical problems, the present invention discloses a method for separating a lignin-carbohydrate complex with intact structure, comprising the following steps:
[0007] S1: crushing the wood fiber raw material, sieving and drying to constant weight to obtain dry powder; then, using benzene alcohol to perform Soxhlet extraction on the wood fiber raw material, and ending the reaction when the solution in the extractor becomes colorless and transparent, and then taking out and drying until the moisture content is less than 1%;
[0008] S2 uses a planetary ball mill to ball mill the solid powder;
[0009] S3: mixing the ball-milled solid powder with 1,4-dioxane, stirring and extracting at room temperature, then centrifuging to separate the solid precipitate, washing with deionized water, and freeze-drying to obtain a primary filter residue;
[0010] S4: Mix the primary residue with acetic acid-sodium acetate buffer and place on a shaker, add xylanase to start the enzymatic hydrolysis reaction. After the reaction is completed, centrifuge to separate the solid residue, wash it with deionized water until it is neutral, and freeze-dry it to obtain a secondary filter residue.
[0011] S5: The secondary residue is mixed with acetic acid-sodium acetate buffer and placed on a shaker, and cellulase is added to start the enzymatic hydrolysis reaction. After the reaction is completed, the solid residue is separated by centrifugation, washed with deionized water until neutral, and freeze-dried to obtain a tertiary filter residue.
[0012] S6 uses 1,4-dioxane aqueous solution to stir and extract the third-level filter residue at room temperature. After the extraction is completed, centrifugal separation is performed, and the recovered supernatant is the first-level filtrate;
[0013] S7 uses a rotary evaporator to concentrate the primary filtrate until the concentrated volume is about 5-7 mL. The obtained concentrate is added dropwise to deionized water, and the precipitate and the milky white supernatant are separated by centrifugation. The product obtained after the precipitate is freeze-dried is R-LCC, and the supernatant is concentrated by rotary evaporation and freeze-dried to obtain S-LCC.
[0014] Preferably, S1 crushes the wood fiber raw material, collects it through a sieve of 40-60 mesh, transfers it to a forced air drying oven at 105°C and dries it to constant weight to obtain a dry powder. Then, Soxhlet extraction is performed on the wood fiber raw material using benzyl alcohol (toluene: ethanol = 2:1), and the reaction is terminated after the solution in the extractor becomes colorless and transparent, and the raw material is taken out and transferred to a forced air drying oven at 105°C to dry it until the moisture content is less than 1%.
[0015] S2 uses a planetary ball mill to ball mill the solid powder. In this application, the ball milling speed is 600 rpm and the ball milling time is 5 h.
[0016] Furthermore, in step S1, the wood fiber raw material is selected from reed, poplar, corn stalks, birch, beech, bamboo and the like.
[0017] Furthermore, in step S3, the mass percentage concentration of 1,4-dioxane used is 96%, and the ratio of the mass of the solid residue to the volume of 1,4-dioxane is 1 g: (15-20) mL.
[0018] Furthermore, in step S3, the extraction time is 72 hours, the solvent is replaced every 24 hours, for a total of three times, and the stirring speed is 300-500 rpm.
[0019] Furthermore, in step S4, the xylanase model used is X2753-50G, the mass ratio of the primary filter residue to the xylanase is 1:1.5, the concentration of the acetic acid-sodium acetate buffer is 0.05M, the pH range is 4.5-5.5, and the enzymolysis time is 48-72h.
[0020] Furthermore, in step S5, the cellulase model used is Celluclast 1.5L, the enzyme loading is 50 FPU / g, the filter paper enzyme activity is 127.5862 FPU / mL, and the enzymatic hydrolysis time and buffer conditions are the same as those in step four.
[0021] Furthermore, in step S6, the 1,4-dioxane aqueous solution is prepared according to a volume ratio of 1,4-dioxane to distilled water of 7:3 to 1:9, the ratio of the mass of the secondary filter residue to the volume of the 1,4-dioxane aqueous solution is 1 g: (15-20) mL, and the extraction conditions are the same as those in step three.
[0022] Furthermore, in step S7, the volume ratio of the concentrated liquid to the deionized water is 1:20, and when the liquid is added dropwise, the deionized water needs to be stirred.
[0023] The present invention also provides a structurally intact lignin-carbohydrate complex obtained by the separation method, which is R-LCC and / or S-LCC.
[0024] Compared with the prior art, the present invention has the following innovative improvements:
[0025] The method of the present invention extracts LCC from the enzymatic residue, and the extraction process is simple, the reaction conditions are mild, and the use of toxic solvents is avoided. The obtained LCC structure is complete, and the three main LCC connecting bonds are well preserved, providing technical support for the application of LCC in the fields of biomedicine and the like. The present invention first reduces the particle size of the raw material by mechanical ball milling, thereby destroying the dense structure of the wood fiber raw material and providing more contact sites for subsequent bio-enzyme treatment. Xylanase is used to destroy the glycosidic bonds of xylan on the main chain of the wood fiber raw material, and the high-polymerization degree of xylan is degraded into low-polymerization degree of xylo-oligosaccharides and monosaccharides, so that the strain and buffering capacity of cellulose to the outside world are weakened, and the subsequent accessibility of cellulose to cellulase is increased, so that the subsequent enzymatic hydrolysis efficiency is improved, and the separation of LCC is promoted. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more specifically illustrate the technical solution of the present invention, the following briefly introduces the drawings required for use in the specific embodiments.
[0027] Figure 1 FT-IR spectra of R-LCC and S-LCC separated by different methods;
[0028] Figure 2 2D NMR spectra of R-LCC and S-LCC isolated by different methods. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Embodiment 1:
[0031] 15g of ball-milled Phragmites australis powder (ball-milled for 5h) and 288mL of 96% 1,4-dioxane solution were placed in a round-bottom flask, and extracted at room temperature for 72h at a stirring speed of 500rpm, with the solvent replaced every 24h. After the extraction, the solid precipitate was collected by centrifugation, washed with deionized water until there was no organic solvent, and then freeze-dried to obtain a primary filter residue;
[0032] Mix 8g of the primary filter residue and 400mL of 0.05M acetic acid-sodium acetate buffer and transfer to a 500mL conical flask. After sealing the flask, transfer to a thermostatic shaker preheated to 50°C and control the oscillation speed at 150rpm. After preheating for 10 minutes, add 12g of xylanase to the conical flask to start the enzymatic hydrolysis reaction. After 72 hours, centrifuge to separate the supernatant and precipitate, wash the solid precipitate with deionized water until it is neutral, and then freeze-dry to obtain the secondary filter residue;
[0033] Using the same method, the secondary filter residue was enzymatically hydrolyzed with Celluclast 1.5L cellulase with an enzyme loading of 50 FPU / g and a filter paper enzyme activity of 127.5862 FPU / mL. After 72 hours, the supernatant and the precipitate were separated by centrifugation, and the solid precipitate was washed with deionized water until neutral and then freeze-dried to obtain the tertiary filter residue.
[0034] Mix the third-grade filter residue and the 1,4-dioxane aqueous solution and transfer them to a 300 mL round-bottom flask. Extract at room temperature for 72 hours with a stirring speed of 500 rpm, and change the solvent every 24 hours. The 1,4-dioxane aqueous solution is prepared according to a volume ratio of 1,4-dioxane to distilled water of 8:2. After each extraction, collect the supernatant by centrifugation, and combine the supernatants of three extractions to form the first-grade filtrate;
[0035] The primary filtrate was concentrated using a rotary evaporator until the concentrated volume was about 7 mL. 140 mL of deionized water was placed on a magnetic stirrer, and the obtained concentrate was added dropwise to the deionized water under stirring to precipitate R-LCC, and the supernatant was rotary evaporated to precipitate S-LCC. After washing with deionized water, two types of LCC were freeze-dried and named R-LCC1 and S-LCC1, respectively.
[0036] The chemical composition of LCC samples was analyzed according to the standard analytical method proposed by the National Renewable Energy Laboratory. TM The PA-1 column and pulsed amperometric detector were used to determine the sugars in the acid hydrolyzate during the analysis. The structural information of LCC was obtained by 2D-HSQC NMR using a Bruker Avance 600 MHz NMR instrument.
[0037] As can be seen from Table 1, the monosaccharide composition of the two LCCs is the same, but the total sugar content is quite different. The main monosaccharide type of R-LCC1 is glucose, accounting for about 11.46%, followed by xylose and galactose; while S-LCC1 is a xylose-rich LCC, followed by galactose and galacturonic acid, and most of the carbohydrates are degraded, which increases the relative proportion of lignin. The 2D-HSQC NMR results show that the two separated LCCs retain the three LCC connecting bonds and have a complete structure.
[0038] Table 1
[0039]
[0040]
[0041] Example 2
[0042] The difference between Example 2 and Example 1 is that corn straw powder is used instead of reed powder, the ratio of the mass of solid residue to the volume of 1,4-dioxane is 1 g:15 mL, and the other parameters are the same as those of Example 1. The two washed and freeze-dried LCCs are named R-LCC2 and S-LCC2, respectively.
[0043] Example 3
[0044] The difference between Example 3 and Example 1 is that bamboo powder is used instead of reed powder, the ratio of the mass of solid residue to the volume of 1,4-dioxane is 1 g:15 mL, and the other parameters are the same as those of Example 1. The two washed and freeze-dried LCCs are named R-LCC3 and S-LCC3, respectively.
[0045] Example 4
[0046] The difference between Example 4 and Example 1 is that the volume ratio of 1,4-dioxane to distilled water is 7:3, and the other parameters are the same as those of Example 1. The two types of LCCs washed and freeze-dried are named R-LCC4 and S-LCC4, respectively.
[0047] Example 5
[0048] The difference between Example 5 and Example 1 is that the volume ratio of 1,4-dioxane to distilled water is 9:1, and the other parameters are the same as those of Example 1. The two types of LCCs washed and freeze-dried are named R-LCC5 and S-LCC5, respectively.
[0049] Comparative Example 1
[0050] The difference between Comparative Example 1 and Example 1 is that only xylanase is used for enzymatic hydrolysis, and cellulase is not used for treatment, and the other parameters are the same as those of Example 1. The two washed and freeze-dried LCCs are named R-LCC6 and S-LCC6, respectively.
[0051] The LCC obtained in Example 1 and Comparative Example 1 were compared by Fourier transform infrared spectroscopy. Figure 1 As shown. Figure 1 It can be seen that 1600cm -1 、1510cm -1 、1420cm -1 The peak at 1735cm is the vibration peak of the benzene ring carbon skeleton, which is a significant characteristic peak of the lignin structural unit, proving the presence of lignin in LCC. -1 The absorption peak at 1035cm is the CO bond stretching in the esterified phenolic acid and acetyl groups associated with xylose or uronic acid of hemicellulose, a feature attributed to the ester bond formed between lignin and carbohydrates in LCC. -1 The absorption peak at 985 cm is a typical signal of hemicellulose. -1 The absorption peak at 875 cm is the characteristic peak of the arabinose side chain. -1 The peak at is the stretching vibration of the β-glycosidic bond. These signals all indicate that the product separated by the method of the present invention is LCC, and the LCC structure is less degraded.
[0052] The LCC samples of Examples 1 to 5 and Comparative Example 1 were characterized by two-dimensional single quantum carbon-hydrogen correlation spectroscopy (2D-HSQC), the linking bond signals were integrated and normalized, and the three LCC linking bond contents obtained were shown in Table 2.
[0053] Table 2
[0054]
[0055]
[0056] Note:
[0057] a: LCC bonds are calculated based on 100 lignin units;
[0058] b: Since the purity of the LCC obtained in Comparative Example 1 is low and its solubility in the deuterated reagent is not large, it cannot be detected by nuclear magnetic resonance, and therefore the phenyl glycosidic bond content cannot be calculated.
[0059] As can be seen from the above table, the NMR signals of the phenyl glycosidic bond, ester bond and ether bond of the LCC samples extracted in Examples 1 to 5 all appear, and the connecting bond structure of the separated LCC remains intact with a high purity.
Claims
1. A method for separating a lignin-carbohydrate complex with intact structure, comprising the following steps: S1 crushes the wood fiber raw material, sieves and dries it to constant weight to obtain dry powder; then, Soxhlet extraction is performed on the wood fiber raw material using benzene alcohol, and the reaction is terminated when the solution in the extractor becomes colorless and transparent, and the raw material is taken out and dried until the moisture content is less than 1%; S2 uses a planetary ball mill to ball mill the solid powder; S3: mixing the ball-milled solid powder with 1,4-dioxane, stirring and extracting at room temperature, then centrifuging to separate the solid precipitate, washing with deionized water, and freeze-drying to obtain a primary filter residue; S4: mixing the primary residue with acetic acid-sodium acetate buffer and placing it on a shaker, adding xylanase to start the enzymatic hydrolysis reaction; after the reaction is completed, centrifuging and separating the solid residue, washing it with deionized water until it is neutral, and freeze-drying it to obtain a secondary filter residue; S5: mixing the secondary residue with acetic acid-sodium acetate buffer and placing it on a shaker, and adding cellulase to start the enzymatic hydrolysis reaction; after the reaction, centrifuging and separating the solid residue, washing it with deionized water until it is neutral, and freeze-drying it to obtain a tertiary filter residue; S6 uses 1,4-dioxane aqueous solution to stir and extract the third-level filter residue at room temperature; after the extraction is completed, centrifugal separation is performed, and the recovered supernatant is the first-level filtrate; S7 uses a rotary evaporator to concentrate the primary filtrate, and the obtained concentrated solution is added dropwise to deionized water, and the precipitate and the milky white supernatant are separated by centrifugation. The product obtained after the precipitate is freeze-dried is R-LCC, and the supernatant is concentrated by rotary evaporation and freeze-dried to obtain S-LCC.
2. The separation method according to claim 1, characterized in that The specific operation of step S1 is: crushing the wood fiber raw material, collecting it through a sieve with a mesh size of 40-60, transferring it to a forced air drying oven at 105°C and drying it to constant weight to obtain a dry powder; then, using benzene alcohol with a ratio of toluene to ethanol = 2:1 to perform Soxhlet extraction on the wood fiber raw material, and terminating the reaction after the solution in the extractor becomes colorless and transparent, taking it out and transferring it to a forced air drying oven at 105°C to dry it until the moisture content is less than 1%.
3. The separation method according to claim 1, characterized in that In step S2, the ball milling speed is 600 rpm and the ball milling time is 3-8 h.
4. The separation method according to claim 1, characterized in that The wood fiber raw material is selected from reed bamboo, poplar, corn stalks, birch, beech and bamboo.
5. The separation method according to claim 1, characterized in that In step S3, the mass percentage concentration of 1,4-dioxane used is 96%, and the ratio of the mass of the solid residue to the volume of 1,4-dioxane is 1g:15-20mL; the extraction time is 72h, the solvent is replaced every 24h, for a total of three times, and the stirring speed is 300-500rpm.
6. The separation method according to claim 1, characterized in that In step S4, the xylanase model used is X2753-50G, the mass ratio of the primary filter residue to the xylanase is 1:1.5, the concentration of the acetic acid-sodium acetate buffer is 0.05M, the pH range is 4.5-5.5, and the enzymolysis time is 48-72h.
7. The separation method according to claim 1, characterized in that In step S5, the cellulase model used is Celluclast 1.5L, the enzyme loading is 50 FPU / g, the filter paper enzyme activity is 127.5862 FPU / mL, and the enzymatic hydrolysis time and buffer conditions are the same as those in step S4.
8. The separation method according to claim 1, characterized in that In step S6, the 1,4-dioxane aqueous solution is prepared according to a volume ratio of 1,4-dioxane to distilled water of 7:3 to 1:9, the mass ratio of the secondary filter residue to the volume of the 1,4-dioxane aqueous solution is 1 g: 15-20 mL, and the extraction conditions are the same as those in step S3.
9. The separation method according to claim 1, characterized in that In step S7, the volume ratio of the concentrated liquid to the deionized water is 1:20, and the deionized water is added dropwise while stirring.
10. The structurally intact lignin-carbohydrate complex obtained by the separation method according to any one of claims 1 to 9, which is R-LCC and / or S-LCC.