Resource utilization method of chromium slag
By performing multiple alkali treatments and microwave reactions on the chromium slag, we successfully achieved the removal of phosphorus and the retention of chromium in the chromium slag, solved the key problem of resource utilization of chromium slag, and realized the resource utilization of chromium, iron and nickel. , and reduces environmental pollution and meets the iron ore standards for steelmaking.
Patent Information
- Application Number
- CN202410783878.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-18
AI Technical Summary
Existing technology makes it difficult to realize resource utilization of all elements in chromium slag, especially the selective extraction and leaching of phosphorus, which results in limited utilization of chromium slag in the steelmaking industry and environmental pollution problems.
By subjecting the chromium slag to primary, secondary and tertiary alkali treatment, filtration and microwave reaction respectively, phosphorus removal and chromium retention are achieved to obtain phosphate and phosphorus-extracted chromium slag, which can be used for steelmaking and recycled Lye to reduce environmental pollution.
The mass percentage of phosphorus in the chromium slag is reduced to less than 0.2%, meeting the iron ore standards for steelmaking, realizing resource utilization of chromium, iron and nickel, eliminating environmental pollution, and is simple to operate and economically feasible.
Smart Images

Figure CN118755950A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource utilization of solid waste, and in particular relates to a resource utilization method of chromium slag. Background Art
[0002] Since the main elements of nickel-iron alloy are iron and nickel, it can provide nickel and iron sources for ternary materials and lithium iron phosphate materials. At the same time, nickel-iron alloy has a high price advantage and is favored by battery positive electrode material manufacturers. As a companion element of nickel, a small amount of chromium will inevitably be doped in nickel-iron alloy. In order to obtain pure nickel salts and iron salts, chromium will be discharged from the nickel-iron production line in the form of chromium slag. However, chromium compounds contained in chromium slag are carcinogens. During the storage and stacking of chromium slag, chromium is easy to leak, causing serious environmental pollution. The reduction, resource utilization and stabilization of chromium slag have always received extensive attention from the government and all sectors of society.
[0003] In terms of resource utilization of chromium slag, "A Hollow Ultralight Ceramic Based on Oil-Based Rock Cuttings and Its Preparation Method" directly mixes ferrochromium slag into raw materials to prepare lightweight ceramsite; "A Method for Cascade Resource Treatment of Calcium-Free Roasted Chromium Slag" selectively reduces iron and chromium compounds in chromium slag to obtain metallic ferrochromium-rich chromium residue, realizing the resource utilization of iron in ferrochromium slag; "A Process for Recycling Chromium-Containing Electroplating Sludge to Prepare Chromium Oxide" extracts chromium from chromium-containing electroplating sludge to prepare sodium dichromate, realizing the resource utilization of chromium in chromium slag. The above patents include conventional ways to recycle chromium slag. The first conventional way is to mix a small proportion of chromium slag into cement and building materials without destroying the composition and structure of the chromium slag, and directly recycle the chromium slag; the second conventional way is to separate high-content elements in the chromium slag to realize the resource utilization of other valuable elements in the chromium slag; the third conventional way is to extract chromium from the chromium slag to prepare chromium salts. The above methods are all for resource utilization of chromium slag. However, the first conventional route has a low doping ratio and limited utilization of chromium slag; the second conventional route has problems such as incomplete separation of chromium from other elements and low utilization of valuable elements; the third conventional route has problems such as large consumption of acid and alkali in the preparation of chromium salts. At the same time, there are no related reports on the resource utilization of all elements of chromium slag.
[0004] The main elements of chromium slag from the nickel-iron alloy production line are Fe (≈33%), P (≈15%), Ni (≈1.35%), and Cr (≈0.65%), among which Fe, Ni, and Cr are the main elements for steelmaking, but P is a harmful element for steelmaking. The requirements for P in steelmaking raw materials are very strict (the standard for iron ore for steelmaking requires the P content to be less than 0.25%, and the iron ore for ironmaking requires the P content to be less than 0.15%. The specific standards are recorded in the "Geological and Mineral Industry Standard of the People's Republic of China DZ / T 0200-2002 Specification for Geological Exploration of Iron-Manganese-Chromium Ore". This standard is the requirement for iron oxide. After converting iron hydroxide into iron oxide, the P content in iron hydroxide is less than 0.2% based on the iron content. It meets the standard). If the P content in chromium slag can be reduced to less than 0.2%, the mixture containing Fe, Ni, and Cr can be used in the steel smelting industry. If the P content cannot be reduced to within the standard range, the mixture containing Fe, Ni, and Cr is still hazardous waste due to the presence of Cr and cannot be effectively utilized. That is to say, the key to realizing resource utilization of chromium slag is to selectively extract P and reduce the P content to below 0.2%. However, the prior art does not disclose any report on selectively extracting and leaching P from chromium slag. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for resource utilization of chromium slag that can utilize all elements in the chromium slag as resources.
[0006] To achieve the above object, in a first aspect of the present invention, the present invention provides a method for resource utilization of chromium slag, the resource utilization method comprising the following steps:
[0007] (1) washing the chromium slag with water and placing it in a primary alkali solution for a first reaction, filtering after the first reaction to obtain a phosphate leachate and a primary alkali-leached chromium slag; cooling and crystallizing the phosphate leachate to obtain a phosphate solid and a mother liquor;
[0008] (2) placing the primary alkali leached chromium residue in a secondary alkali solution for a second reaction, and filtering after the second reaction is completed to obtain a secondary alkali leaching solution and a secondary alkali leached chromium residue;
[0009] (3) placing the secondary alkaline leaching chromium residue in the tertiary alkaline solution for microwave reaction, filtering after the microwave reaction is completed, and obtaining the tertiary alkaline leaching solution and the phosphorus-extracting chromium residue.
[0010] In the resource utilization method of chromium slag provided by the present invention, the chromium slag is subjected to a primary alkali leaching treatment, and phosphorus in the chromium slag is leached into the liquid phase in the form of phosphate, while chromium is retained in the solid phase in the form of primary alkali leached chromium slag; the phosphate leachate after the primary alkali leaching treatment is cooled and crystallized to obtain phosphate, thereby realizing resource utilization of phosphorus; then the primary alkali leached chromium slag is subjected to a secondary alkali leaching treatment and a tertiary alkali leaching treatment respectively, thereby realizing deep phosphorus extraction of the chromium slag, and the mass percentage of phosphorus in the obtained phosphorus extraction chromium slag is less than 0.2%, so the obtained phosphorus extraction chromium slag can be used as iron ore for steelmaking, thereby realizing resource utilization of iron, nickel and chromium. Moreover, in the resource utilization method provided by the present invention, the obtained mother liquor, secondary alkali leaching liquid and tertiary alkali leaching liquid can be returned to the primary alkali solution for repeated utilization, thereby realizing the recycling of the alkali solution, and achieving an environmentally friendly and environmentally friendly resource utilization method.
[0011] In one embodiment, the chromium slag includes chromium slag produced in the process of producing nickel salt and / or iron salt from nickel-iron alloy.
[0012] In one embodiment, based on the chromium slag, the mass percentage of the iron element is 30-40%, the mass percentage of the phosphorus element is 12-18%, the mass percentage of the nickel element is 1-1.7%, and the mass percentage of the chromium element is 0.5-2.0%.
[0013] The present invention has found that the elements in the chromium slag generated in the process of producing nickel salts and / or iron salts from nickel-iron alloys mainly include iron, phosphorus, nickel and chromium, and the main phases are hydrated iron phosphate and hydroxy iron phosphate; after being treated by the resource utilization method provided by the present invention, phosphate can be recovered, and the mass percentage of phosphorus in the obtained phosphorus-extracting chromium slag is less than 0.2%, which can be used as iron ore for steelmaking; thereby achieving the comprehensive resource utilization of all elements in the chromium slag generated in the process of producing nickel salts and / or iron salts from nickel-iron alloys.
[0014] In one embodiment, the ratio of the sum of the molar numbers of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:(1-5).
[0015] In one embodiment, the ratio of the sum of the molar numbers of positive charges of metal ions in the primary alkaline leaching chromium slag to the molar number of hydroxide in the secondary alkaline solution is 1:(1-8).
[0016] In one embodiment, the ratio of the sum of the molar numbers of positive charges of metal ions in the secondary alkaline leaching chromium slag to the molar number of hydroxide in the tertiary alkaline solution is 1:(1-8).
[0017] The present invention has found that, whether it is the ratio of the sum of the molar numbers of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution, the ratio of the sum of the molar numbers of positive charges of metal ions in the primary alkali leaching chromium slag to the molar number of hydroxide in the secondary alkali solution, or the ratio of the sum of the molar numbers of positive charges of metal ions in the secondary alkali leaching chromium slag to the molar number of hydroxide in the tertiary alkali solution, when all three are within the range given by the present invention, it can be ensured that when the corresponding solid is placed in the alkali solution, the alkali solution can be alkaline, thereby achieving phosphorus removal.
[0018] It should be noted that the metal ions and their contents in the chromium slag and the alkali-leached chromium slag are tested by the ICP method. The metal ions and their contents are obtained by the ICP test, and then the sum of the molar numbers of positive charges of the metal ions in the corresponding chromium slag and the alkali-leached chromium slag is calculated.
[0019] Specifically, the ratio of the sum of the molar numbers of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:(1-5) as an example for explanation. For example, after detection, the chromium slag contains divalent metal elements nickel n1 mol, magnesium n2 mol, ..., X nx mol, trivalent metal elements iron n3 mol, chromium n4 mol, ..., Y ny mol, and tetravalent metal element Z nz mol. Then the sum of the molar numbers of positive charges of metal ions in the chromium slag M is 2*(n1+n2+...+nx)+3*(n3+n4+...+ny)+4nz mol, and the molar number of hydroxide in the primary alkali solution is (1-5)M; the ratio of the sum of the molar numbers of positive charges of metal ions in the primary alkali leaching chromium slag to the molar number of hydroxide in the secondary alkali solution or the ratio of the sum of the molar numbers of positive charges of metal ions in the secondary alkali leaching chromium slag to the molar number of hydroxide in the tertiary alkali solution is applicable by analogy.
[0020] The present invention has no special requirements for the primary alkali solution, the secondary alkali solution and the tertiary alkali solution, and any solution that can ionize hydroxide in an aqueous solution can achieve the effect of the present invention.
[0021] In one embodiment, the solutes in the primary alkali solution, the secondary alkali solution and the tertiary alkali solution independently include at least one of liquid ammonia, ammonia water, sodium hydroxide, potassium hydroxide, magnesium hydroxide and calcium hydroxide; and the solvent in the primary alkali solution, the secondary alkali solution and the tertiary alkali solution includes water.
[0022] The present invention uses different solutes in the alkali solution, and the phosphates obtained after one alkali leaching treatment are also different accordingly. For example, if the solute is sodium hydroxide, the phosphate obtained is trisodium phosphate dodecahydrate; if the solute is magnesium hydroxide, the phosphate obtained is magnesium phosphate, and so on.
[0023] In one embodiment, the primary alkali solution, the secondary alkali solution and the tertiary alkali solution are selected from aqueous sodium hydroxide solution.
[0024] The present invention has found that when the primary alkali solution, the secondary alkali solution and the tertiary alkali solution are further selected from the sodium hydroxide aqueous solution, the obtained phosphate is trisodium phosphate dodecahydrate, which not only has relatively excellent stability but also has a wider application range.
[0025] In one embodiment, the liquid-to-solid ratios of the chromium slag and the primary alkali solution, the primary alkali leaching chromium slag and the secondary alkali solution, and the secondary alkali leaching chromium slag and the tertiary alkali solution are each independently (2-6) mL / g.
[0026] The present invention has found that when the liquid-to-solid ratio in the three alkali leaching processes is further selected to be (2-6) mL / g, phosphorus in the chromium slag can be better removed and the mass percentage of phosphorus in the final phosphorus extraction chromium slag can be reduced.
[0027] In one embodiment, the environments of the first reaction, the second reaction and the microwave reaction are each independently a closed environment, a reduced pressure environment or an inert gas environment.
[0028] The present invention has been found that ensuring that the reaction environment during the alkali leaching process is a closed environment, a reduced pressure environment or an inert gas environment can prevent the trivalent chromium in the alkali leaching process from being oxidized to hexavalent chromium by air, thereby preventing the oxidized hexavalent chromium from dissolving in the alkali solution, resulting in difficulty in separating the subsequent chromium and phosphorus elements in the alkali solution, leading to the problem of excessive chromium content in the phosphate product; by carrying out alkali leaching treatment under the reaction environment provided by the present invention, chromium can maintain a trivalent state, and effective separation of chromium and phosphorus can be achieved. Specifically, the trivalent chromium can be completely retained in the solid phase, and the phosphorus can be fully extracted into the liquid phase, thereby improving the full-element resource utilization efficiency and effect of the chromium slag.
[0029] In one embodiment, the closed environment includes a closed reactor.
[0030] In one embodiment, the inert gas used in the inert gas environment includes nitrogen and a rare gas.
[0031] In one embodiment, the temperature of the first reaction is 60-90° C., and the time of the first reaction is 2-4 hours.
[0032] In one embodiment, the temperature of the second reaction is 60-90° C., and the time of the second reaction is 2-4 hours.
[0033] The present invention has found that when the temperature and time of the first reaction and the second reaction are further selected within the above range, phosphorus leaching can be better achieved, and the mass percentage of phosphorus in the subsequent phosphorus extraction chromium slag can be reduced, thereby achieving efficient resource utilization of the chromium slag.
[0034] In one embodiment, in step (3), the microwave reaction time is 5-20 min, the microwave reaction power is 500-800 W, and the microwave reaction temperature is 60-120° C.
[0035] The present invention has found that when a microwave reaction is introduced into the three alkali leaching processes and the time, power and temperature of the microwave reaction are selected within the range given by the present invention, phosphorus can be deeply extracted, the mass percentage of phosphorus in the phosphorus extraction chromium slag can be better reduced, and an excellent resource utilization effect can be achieved.
[0036] The present invention has no special requirements for the filtering method, as long as the solid and the liquid can be separated; for example, the filtering method of the present invention can be any one of pressure filtration, centrifugation, and sedimentation.
[0037] In a second aspect of the present invention, the present invention provides a phosphorus-extracting chromium slag, wherein the phosphorus-extracting chromium slag is prepared by the resource utilization method of chromium slag of the present invention.
[0038] The mass percentage of phosphorus in the phosphorus-extracting chromium slag provided by the invention is less than 0.2%, and the iron ore can be used for steelmaking, thereby realizing efficient utilization of the phosphorus-extracting chromium slag.
[0039] In the third aspect of the present invention, the present invention provides the use of the phosphorus-chromium extracting slag in steel smelting.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] In the resource utilization method of chromium slag provided by the present invention, by subjecting the chromium slag to a primary alkali leaching treatment, phosphorus in the chromium slag is leached into the liquid phase in the form of phosphate, and chromium is retained in the solid phase in the form of primary alkali leached chromium slag; the phosphate leachate after the primary alkali leaching treatment is cooled and crystallized to obtain phosphate, thereby realizing resource utilization of phosphorus; then the primary alkali leached chromium slag is subjected to secondary alkali leaching treatment and tertiary alkali leaching treatment respectively to achieve deep phosphorus extraction of the chromium slag, and the mass percentage of phosphorus in the obtained phosphorus extraction chromium slag is less than 0.2%, so the obtained phosphorus extraction chromium slag can be used as iron ore for steelmaking, thereby realizing resource utilization of iron, nickel and chromium. At the same time, in the resource utilization method provided by the present invention, the obtained mother liquor, secondary alkali leaching liquid and tertiary alkali leaching liquid can be returned to the primary alkali liquor to realize the recycling of the alkali liquor, and in addition to the two products of phosphate and phosphorus extraction chromium slag, no other waste residue and waste gas will be generated, so the present invention not only eliminates the environmental pollution of the chromium slag, but also does not generate other pollution, that is, it achieves an environmentally friendly and environmentally friendly resource utilization method. Moreover, the product phosphate and iron ore precursor of the method for resource utilization of chromium slag provided by the present invention are bulk commodities, have wide application paths and high market value, that is, strong economic feasibility; at the same time, the method for resource utilization of chromium slag provided by the present invention is simple to operate, has no special requirements on conditions, and is conducive to actual production. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1This is a schematic diagram of the process flow of the method for resource utilization of chromium slag provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0043] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0044] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0045] Example 1
[0046] The embodiment of the present invention provides a method for resource utilization of chromium slag, and the process flow diagram of the resource utilization method is as follows: Figure 1 As shown, the specific steps include:
[0047] (1) taking 100 g of chromium slag (calculated on the basis of the chromium slag, the mass percentage of iron is 33.36%, the mass percentage of phosphorus is 15.29%, the mass percentage of nickel is 1.35%, and the mass percentage of chromium is 0.65%), adding it to 1 L of water and stirring it at room temperature to remove soluble impurities in the chromium slag; then adding the washed chromium slag to 300 mL of primary alkali solution (the primary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 75 g; the ratio of the sum of the molar number of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:3), introducing a small amount of nitrogen into the reaction environment to allow the first reaction to proceed under anoxic conditions, and stirring the reaction at 80° C. for 3 h. After the stirring reaction is completed, filtering is performed to obtain a sodium phosphate leaching solution and a primary alkali leached chromium slag;
[0048] The sodium phosphate leachate is cooled to 45°C, sodium phosphate seed crystals are added for cooling and crystallization, and then filtered, the solid is collected and dried at 40°C to obtain a trisodium phosphate product;
[0049] (2) adding 32 g of the primary alkali leached chromium slag to 150 mL of secondary alkali solution (the secondary alkali solution is a sodium hydroxide aqueous solution, the mass of the sodium hydroxide is 7.5 g; the ratio of the sum of the molar number of positive charges of metal ions in the primary alkali leached chromium slag to the molar number of hydroxide in the secondary alkali solution is 1:4), introducing a small amount of nitrogen into the reaction environment to allow the second reaction to proceed under anoxic conditions, and stirring the reaction at 80° C. for 3 h. After the stirring reaction is completed, filtering is performed to obtain a secondary alkali leaching solution and a secondary alkali leached chromium slag;
[0050] (3) 29 g of secondary alkaline leaching chromium slag was added into 150 mL of tertiary alkaline solution (the tertiary alkaline solution was a sodium hydroxide aqueous solution with a mass of 7.5 g of sodium hydroxide; the ratio of the sum of the molar number of positive charges of metal ions in the secondary alkaline leaching chromium slag to the molar number of hydroxide in the tertiary alkaline solution was 1:6), and microwave reaction was carried out in a closed environment. The microwave reaction time was 15 min, the power was 600 W, and the temperature was 80°C. After the microwave reaction was completed, the tertiary alkaline leaching solution and phosphorus-extracted chromium slag were obtained by filtration.
[0051] Example 2
[0052] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (2), 32g of primary alkali-leached chromium slag is added to 150mL of secondary alkali solution (the secondary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 6g; the ratio of the sum of the molar number of positive charge of metal ions in the primary alkali-leached chromium slag to the molar number of hydroxide in the secondary alkali solution is 1:3.2); and in step (3), 30g of secondary alkali-leached chromium slag is added to 150mL of tertiary alkali solution (the tertiary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 6g; the ratio of the sum of the molar number of positive charge of metal ions in the secondary alkali-leached chromium slag to the molar number of hydroxide in the tertiary alkali solution is 1:5).
[0053] Example 3
[0054] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (2), 32g of primary alkali-leached chromium slag is added to 150mL of secondary alkali solution (the secondary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 10g; the ratio of the sum of the molar number of positive charge of metal ions in the primary alkali-leached chromium slag to the molar number of hydroxide in the secondary alkali solution is 1:5.3); and in step (3), 28g of secondary alkali-leached chromium slag is added to 150mL of tertiary alkali solution (the tertiary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 10g; the ratio of the sum of the molar number of positive charge of metal ions in the secondary alkali-leached chromium slag to the molar number of hydroxide in the tertiary alkali solution is 1:8).
[0055] Example 4
[0056] (1) 100 g of chromium slag (calculated as chromium slag, the mass percentage of iron is 33.36%, the mass percentage of phosphorus is 15.29%, the mass percentage of nickel is 1.35%, and the mass percentage of chromium is 0.65%) is added to 1 L of water and stirred at room temperature to remove soluble impurities in the chromium slag; then the washed chromium slag is added to 300 mL of primary alkali solution (the primary alkali solution is a potassium hydroxide aqueous solution, the mass of potassium hydroxide is 105 g; the ratio of the sum of the molar number of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:3), a small amount of nitrogen is introduced into the reaction environment to allow the first reaction to proceed under anoxic conditions, and the reaction is stirred at 80° C. for 3 h. After the stirring reaction is completed, the solution is filtered to obtain potassium phosphate leaching solution and primary alkali leached chromium slag;
[0057] The potassium phosphate leachate is cooled to 45°C, potassium phosphate seed crystals are added for cooling and crystallization, and then filtered, the solid is collected and dried at 40°C to obtain a potassium phosphate product;
[0058] (2) adding 34 g of the primary alkali leached chromium slag to 150 mL of secondary alkali solution (the secondary alkali solution is a potassium hydroxide aqueous solution, the mass of potassium hydroxide is 10 g; the ratio of the sum of the molar number of positive charges of metal ions in the primary alkali leached chromium slag to the molar number of hydroxide in the secondary alkali solution is 1:4), introducing a small amount of nitrogen into the reaction environment to allow the second reaction to proceed under anoxic conditions, and stirring the reaction at 80° C. for 3 h. After the stirring reaction is completed, filtering is performed to obtain a secondary alkali leaching solution and a secondary alkali leached chromium slag;
[0059] (3) 31 g of secondary alkaline leaching chromium slag was added into 150 mL of tertiary alkaline solution (the tertiary alkaline solution was a potassium hydroxide aqueous solution with a mass of 10 g of potassium hydroxide; the ratio of the sum of the molar number of positive charges of metal ions in the secondary alkaline leaching chromium slag to the molar number of hydroxide in the tertiary alkaline solution was 1:6), and microwave reaction was carried out in a closed environment. The microwave reaction time was 15 min, the power was 600 W, and the temperature was 80°C. After the microwave reaction was completed, the tertiary alkaline leaching solution and phosphorus-extracted chromium slag were obtained by filtration.
[0060] Example 5
[0061] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (1), the reaction is stirred at 60° C. for 3 hours.
[0062] Example 6
[0063] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (1), the reaction is stirred at 50° C. for 4 hours.
[0064] Example 7
[0065] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (1), the reaction is stirred at 100° C. for 4 hours.
[0066] Example 8
[0067] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (3), the time of microwave reaction is 5 minutes, the power is 800 W, and the temperature of microwave reaction is 60°C.
[0068] Example 9
[0069] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (3), the time of microwave reaction is 20 minutes, the power is 500 W, and the temperature of microwave reaction is 120°C.
[0070] Example 10
[0071] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (3), the microwave reaction time is 15 minutes and the power is 300W.
[0072] Embodiment 11
[0073] The embodiment of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and Example 1 is that in step (3), the microwave reaction time is 15 minutes and the power is 900W.
[0074] Comparative Example 1
[0075] The comparative example of the present invention provides a method for resource utilization of chromium slag, and the resource utilization method of chromium slag comprises the following steps:
[0076] (1) taking 100 g of chromium slag (calculated on the basis of the chromium slag, the mass percentage of iron is 33.36%, the mass percentage of phosphorus is 15.29%, the mass percentage of nickel is 1.35%, and the mass percentage of chromium is 0.65%), adding it to 1 L of water and stirring it at room temperature to remove soluble impurities in the chromium slag; then adding the washed chromium slag to 300 mL of primary alkali solution (the primary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 75 g; the ratio of the sum of the molar number of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:3), introducing a small amount of nitrogen into the reaction environment to allow the first reaction to proceed under anoxic conditions, and stirring the reaction at 80° C. for 3 h. After the stirring reaction is completed, filtering is performed to obtain a sodium phosphate leaching solution and a primary alkali leached chromium slag;
[0077] The sodium phosphate leachate is cooled to 45°C, sodium phosphate seed crystals are added for cooling and crystallization, and then filtered, the solid is collected and dried at 40°C to obtain a trisodium phosphate product;
[0078] (2) adding 32 g of the primary alkali leached chromium slag to 150 mL of secondary alkali solution (the secondary alkali solution is a sodium hydroxide aqueous solution, the mass of the sodium hydroxide is 7.5 g; the ratio of the sum of the molar number of positive charges of metal ions in the primary alkali leached chromium slag to the molar number of hydroxide in the secondary alkali solution is 1:4), introducing a small amount of nitrogen into the reaction environment to allow the second reaction to proceed under anoxic conditions, and stirring the reaction at 80° C. for 3 h. After the stirring reaction is completed, filtering is performed to obtain a secondary alkali leaching solution and a secondary alkali leached chromium slag;
[0079] (3) 29 g of secondary alkaline leaching chromium slag is added to 150 mL of tertiary alkaline solution (the tertiary alkaline solution is a sodium hydroxide aqueous solution with a mass of 7.5 g of sodium hydroxide; the ratio of the sum of the molar number of positive charges of metal ions in the secondary alkaline leaching chromium slag to the molar number of hydroxide in the tertiary alkaline solution is 1:6), a small amount of nitrogen is introduced into the reaction environment to allow the reaction to proceed under anaerobic conditions, and the reaction is stirred at 80° C. for 3 h. After the stirring reaction is completed, the mixture is filtered to obtain the tertiary alkaline leaching solution and phosphorus-extracting chromium slag.
[0080] Comparative Example 2
[0081] The comparative example of the present invention provides a method for resource utilization of chromium slag. The only difference between the method for resource utilization of chromium slag and comparative example 1 is that in step (2), 32g of primary alkali leached chromium slag is added to 150mL of secondary alkali solution (the secondary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 15g; the ratio of the sum of the molar number of positive charge of metal ions in the primary alkali leached chromium slag to the molar number of hydroxide in the secondary alkali solution is 1:8); and in step (3), 28g of secondary alkali leached chromium slag is added to 150mL of tertiary alkali solution (the tertiary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 10g; the ratio of the sum of the molar number of positive charge of metal ions in the secondary alkali leached chromium slag to the molar number of hydroxide in the tertiary alkali solution is 1:8).
[0082] Comparative Example 3
[0083] The comparative example of the present invention provides a method for resource utilization of chromium slag, and the resource utilization method comprises the following steps:
[0084] (1) taking 100 g of chromium slag (calculated on the basis of the chromium slag, the mass percentage of iron is 33.36%, the mass percentage of phosphorus is 15.29%, the mass percentage of nickel is 1.35%, and the mass percentage of chromium is 0.65%), adding it to 1 L of water and stirring it at room temperature to remove soluble impurities in the chromium slag; then adding the washed chromium slag to 300 mL of primary alkali solution (the primary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 75 g; the ratio of the sum of the molar number of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:3), and performing microwave reaction in a closed environment, the microwave reaction time is 15 min, the power is 600 W, the temperature is 80° C., filtering after the microwave reaction is completed, and obtaining sodium phosphate leaching solution and primary alkali leached chromium slag;
[0085] The sodium phosphate leachate is cooled to 45°C, sodium phosphate seed crystals are added for cooling and crystallization, and then filtered, the solid is collected and dried at 40°C to obtain a trisodium phosphate product;
[0086] (2) adding 32 g of the primary alkali leached chromium slag to 150 mL of secondary alkali solution (the secondary alkali solution is a sodium hydroxide aqueous solution, the mass of the sodium hydroxide is 7.5 g; the ratio of the sum of the molar number of positive charges of metal ions in the primary alkali leached chromium slag to the molar number of hydroxide in the secondary alkali solution is 1:4), introducing a small amount of nitrogen into the reaction environment to allow the second reaction to proceed under anoxic conditions, and stirring the reaction at 80° C. for 3 h. After the stirring reaction is completed, filtering is performed to obtain a secondary alkali leaching solution and a secondary alkali leached chromium slag;
[0087] (3) 29 g of secondary alkaline leaching chromium slag is added to 150 mL of tertiary alkaline solution (the tertiary alkaline solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 7.5 g; the ratio of the sum of the molar number of positive charges of metal ions in the secondary alkaline leaching chromium slag to the molar number of hydroxide in the tertiary alkaline solution is 1:6), a small amount of nitrogen is introduced into the reaction environment to allow the third reaction to proceed under anoxic conditions, and the reaction is stirred at 80° C. for 3 h. After the stirring reaction is completed, the reaction is filtered to obtain the tertiary alkaline leaching solution and phosphorus-extracting chromium slag.
[0088] Comparative Example 4
[0089] The comparative example of the present invention provides a method for resource utilization of chromium slag, and the resource utilization method comprises the following steps:
[0090] (1) taking 100 g of chromium slag (calculated on the basis of the chromium slag, the mass percentage of iron is 33.36%, the mass percentage of phosphorus is 15.29%, the mass percentage of nickel is 1.35%, and the mass percentage of chromium is 0.65%), adding it to 1 L of water and stirring it at room temperature to remove soluble impurities in the chromium slag; then adding the washed chromium slag to 300 mL of primary alkali solution (the primary alkali solution is a sodium hydroxide aqueous solution, the mass of sodium hydroxide is 75 g; the ratio of the sum of the molar number of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:3), introducing a small amount of nitrogen into the reaction environment to allow the first reaction to proceed under anoxic conditions, and stirring the reaction at 80° C. for 3 h. After the stirring reaction is completed, filtering is performed to obtain a sodium phosphate leaching solution and a primary alkali leached chromium slag;
[0091] The sodium phosphate leachate is cooled to 45°C, sodium phosphate seed crystals are added for cooling and crystallization, and then filtered, the solid is collected and dried at 40°C to obtain a trisodium phosphate product;
[0092] (2) adding 32 g of the primary alkali leached chromium residue to 150 mL of secondary alkali solution (the secondary alkali solution is a sodium hydroxide aqueous solution, the mass of the sodium hydroxide is 7.5 g; the ratio of the sum of the molar number of positive charges of metal ions in the primary alkali leached chromium residue to the molar number of hydroxide in the secondary alkali solution is 1:4), and performing microwave reaction in a closed environment, the microwave reaction time is 15 min, the power is 600 W, the temperature is 80° C. After the microwave reaction is completed, filtering is performed to obtain a secondary alkali leaching solution and a secondary alkali leached chromium residue;
[0093] (3) 28 g of secondary alkaline leaching chromium slag is added to 150 mL of tertiary alkaline solution (tertiary alkaline solution is a sodium hydroxide aqueous solution with a mass of 7.5 g of sodium hydroxide; the ratio of the sum of the molar number of positive charges of metal ions in the secondary alkaline leaching chromium slag to the molar number of hydroxide in the tertiary alkaline solution is 1:6.5), a small amount of nitrogen is introduced into the reaction environment to allow the reaction to proceed under anaerobic conditions, and the reaction is stirred at 80° C. for 3 h. After the stirring reaction is completed, the mixture is filtered to obtain the tertiary alkaline leaching solution and phosphorus-extracting chromium slag.
[0094] Effect example
[0095] Effect Examples of the Invention The parameters of the phosphate and phosphorus-extracting chromium slag prepared by the resource utilization method of chromium slag provided in Examples 1-11 and Comparative Examples 1-4 are tested, wherein:
[0096] Purity of phosphate = weight of phosphate dodecahydrate / weight of solid phosphate product obtained in step (1) * 100%;
[0097] Phosphorus yield = [1-phosphorus content in phosphorus-extracting chromium slag*weight of phosphorus-extracting chromium slag / (phosphorus content in chromium slag*weight of chromium slag)]*100%;
[0098] The obtained results are shown in Table 1;
[0099] Table 1
[0100]
[0101] As can be seen from Table 1, when the resource utilization method provided by the present invention is adopted, the comprehensive utilization of all elements in the chromium slag can be effectively achieved, wherein the purity of the obtained phosphate is above 98.5%, the yield of phosphorus is above 99.43%, and the obtained sodium phosphate product meets the standard of "HG / T2517-2009 Industrial Trisodium Phosphate" and can be directly used as industrial trisodium phosphate; the mass percentage of phosphorus in the phosphorus-extracting chromium slag is below 0.20%, and the phosphorus-extracting chromium slag meets the industrial index of iron ore for steelmaking (DZ / T0200-2002), and can be used as a steelmaking raw material later;
[0102] It can be seen from Examples 1-3 that the ratio of the sum of the molar number of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the alkali solution will affect the purity of the sodium phosphate product and the phosphorus yield to a certain extent, and will also have a certain impact on the mass percentage of phosphorus in the phosphorus extraction chromium slag; It can be seen from Examples 1 and 5-11 that the reaction parameters in the resource utilization process will affect the purity of the sodium phosphate product and the phosphorus yield and the mass percentage of phosphorus in the phosphorus extraction chromium slag;
[0103] It can be seen from Example 1 and Comparative Example 1 that when microwave treatment is not introduced in the third alkali leaching treatment, the mass percentage of phosphorus in the obtained phosphorus-extracting chromium slag is significantly increased, which is 2.5 times higher than that in Example 1, and does not meet the DZ / T0200-2002 industrial index; it can be seen from Example 1 and Comparative Example 2 that when microwave treatment is not introduced in the third alkali leaching treatment, even if the amount of sodium hydroxide added in the second alkali leaching treatment and the third alkali leaching treatment is increased, the corresponding dephosphorization effect cannot be achieved, and the mass percentage of phosphorus in the phosphorus-extracting chromium slag in Comparative Example 2 is increased by 1.8 times compared with Example 1; it can be seen from Example 1 and Comparative Examples 3-4 that when microwave reaction is not introduced in the third alkali leaching treatment, but introduced in the first alkali leaching treatment or the second alkali leaching treatment, the phosphorus content in the phosphorus-extracting chromium slag cannot be effectively reduced.
Claims
1. A method for resource utilization of chromium slag, It is characterized in that The resource utilization method comprises the following steps: (1) washing the chromium slag with water and placing it in a primary alkali solution for a first reaction, filtering after the first reaction to obtain a phosphate leachate and a primary alkali-leached chromium slag; cooling and crystallizing the phosphate leachate to obtain a phosphate solid and a mother liquor; (2) placing the primary alkali leached chromium residue in a secondary alkali solution for a second reaction, and filtering after the second reaction is completed to obtain a secondary alkali leaching solution and a secondary alkali leached chromium residue; (3) placing the secondary alkaline leaching chromium residue in the tertiary alkaline solution for microwave reaction, filtering after the microwave reaction is completed, and obtaining the tertiary alkaline leaching solution and the phosphorus-extracting chromium residue.
2. The resource utilization method according to claim 1, It is characterized in that The chromium slag includes chromium slag produced in the process of producing nickel salt and / or iron salt from nickel-iron alloy.
3. The resource utilization method according to claim 1, It is characterized in that Calculated in chromium slag, the mass percentage of the iron element is 30-40%, the mass percentage of the phosphorus element is 12-18%, the mass percentage of the nickel element is 1-1.7%, and the mass percentage of the chromium element is 0.5-2.0%.
4. The resource utilization method according to claim 1, It is characterized in that The ratio of the sum of the molar number of positive charges of metal ions in the chromium slag to the molar number of hydroxide in the primary alkali solution is 1:(1-5); And / or, the ratio of the sum of the molar number of positive charges of metal ions in the primary alkaline leaching chromium slag to the molar number of hydroxide in the secondary alkaline solution is 1:(1-8); And / or, the ratio of the sum of the molar numbers of positive charges of metal ions in the secondary alkaline leaching chromium slag to the molar number of hydroxide in the tertiary alkaline solution is 1:(1-8).
5. The resource utilization method according to claim 1, It is characterized in that The liquid-to-solid ratios of the chromium slag and the primary alkali solution, the primary alkali-leached chromium slag and the secondary alkali solution, and the secondary alkali-leached chromium slag and the tertiary alkali solution are each independently (2-6) mL / g.
6. The resource utilization method according to claim 1, It is characterized in that The environments of the first reaction, the second reaction and the microwave reaction are independently a closed environment, a reduced pressure environment or an inert gas environment.
7. The resource utilization method according to claim 1, It is characterized in that The temperature of the first reaction is 60-90°C, and the time of the first reaction is 2-4h; And / or, the temperature of the second reaction is 60-90° C., and the time of the second reaction is 2-4 hours.
8. The resource utilization method according to claim 1, It is characterized in that In step (3), the microwave reaction time is 5-20 min, the microwave reaction power is 500-800 W, and the microwave reaction temperature is 60-120° C.
9. A phosphorus-chromium slag, It is characterized in that The phosphorus-extracting chromium slag is prepared by the resource utilization method of chromium slag as described in any one of claims 1 to 8 of the present invention.
10. Use of the phosphorus-chromium slag as claimed in claim 9 in steel smelting.
Citation Information
Patent Citations
Acid leaching pretreatment method for extracting chromium from chromium residues
CN111139359A
Cooperative treatment method of chromium-containing electroplating waste liquid and electroplating cleaning water
CN111646598A
Method for selectively separating zinc, chromium and iron and recovering multiple metals in electroplating sludge
CN114752766A
Process for making chromium-nickel steels in bof
RU1786091C