Regenerated rare earth modified high-conductivity 6101 aluminum alloy material and preparation method thereof

By adding regenerated rare earth elements Sm or La to 6101 aluminum alloy to form Mg-Sm or Mg-La master alloy, combined with specific heat treatment and rolling deformation process, the problem of material strength and conductivity balance is solved, and low-cost, The preparation of high-performance 6101 aluminum alloy materials is suitable for new energy vehicles and other fields.

CN118756016AActive Publication Date: 2024-10-11INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202411244301.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-10-11
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The existing 6101 aluminum alloy material is difficult to achieve a balance between improving strength and conductivity, and the high cost of rare earth elements limits its application in fields such as new energy vehicles, electric power, and rail transportation.

Method used

The regenerated rare earth elements Sm or La are used to extract the rare earth elements in the rare earth magnetic waste through Mg element as a collecting agent to form Mg-Sm or Mg-La master alloy. Combined with specific heat treatment and rolling deformation processes, low-cost, Highly conductive 6101 aluminum alloy material.

Benefits of technology

It achieves the high strength and high conductivity of 6101 aluminum alloy material, with tensile strength ≥210 MPa and conductivity ≥58% IACS. It also reduces production costs and provides a way to recycle secondary rare earth metal resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756016A_ABST
    Figure CN118756016A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of secondary rare earth recycling and light high-conductivity metal materials, and particularly relates to a regenerated rare earth modified high-conductivity 6101 aluminum alloy material and a preparation method thereof. The aluminum alloy comprises the following components in percentage by mass: 0.03-0.3% of regenerated rare earth element Sm or La, 0.05-0.1% of iron Fe and the balance of 6101 aluminum alloy. The method comprises the following steps: firstly, extracting rare earth elements Sm and La in the rare earth magnetic waste by using Mg element to prepare Mg-Sm and Mg-La intermediate alloys; secondly, elements Si, Fe and Mg are sequentially added into the aluminum melt, and the alloy melt is stirred and subjected to heat preservation; then, a refining agent and argon are introduced into the melt for refining; then, rare earth elements Sm or La are added into the alloy melt in the form of Mg-Sm or Mg-La intermediate alloy, after stirring and standing, a uniform melt is obtained, and then the uniform melt is cast into an ingot; and finally, the cast ingot is subjected to homogenization, solid solution quenching, rolling deformation and aging treatment in sequence.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of secondary rare earth recycling and lightweight high-conductivity metal materials, specifically relating to a high-conductivity 6101 aluminum alloy material modified with recycled rare earth and its preparation method. Background Technology

[0002] Aluminum has the highest electrical conductivity after silver, copper, and gold, with a density that is 25.7% of silver, 30.3% of copper, and 13.9% of gold. Moreover, aluminum is significantly cheaper than these precious metals. Therefore, developing lightweight, high-strength, and highly conductive aluminum alloys is crucial for promoting the development of industries such as rail transportation, power, and new energy vehicles. 6101 is a low-alloyed Al-Mg-Si aluminum alloy. Compared to other 6XXX series aluminum alloys, 6101 aluminum alloy has higher specific strength, stronger corrosion resistance, excellent electrical conductivity, and good heat treatability and formability. In recent years, the rapid development of industries such as new energy electric vehicles, power, and rail transportation has placed more stringent demands on the conductivity, mechanical properties, corrosion resistance, and manufacturing cost of 6101 aluminum alloy. According to relevant patents (such as: Publication No. CN105950893B), every 0.1% increase in the conductivity of aluminum conductors used in electrical engineering nationwide can reduce electricity loss by 10 billion kilowatt-hours annually. In recent years, the composition optimization design and preparation technology of 6101 aluminum alloy have attracted widespread attention and research from aluminum alloy material scientists and technicians.

[0003] Patents (CN118143074A, CN110093536B, CN115740057A) disclose high-conductivity 6101 aluminum alloy coils for new energy applications, battery conductors, and power supply for new energy vehicles, respectively, and their preparation methods. The preparation methods mainly include: preparing wire rods according to the national standard composition of 6101 aluminum alloy, continuous extrusion of wire rods, and aging treatment of extruded profiles. The extrusion process is optimized to improve material performance, resulting in aluminum busbar coils for new energy applications with high conductivity, The tensile strength and elongation can be 57.8% IACS, 190 MPa, and 13.5%, respectively. The conductivity, tensile strength, yield strength, and elongation of the obtained aluminum strip for battery conductors can be 58.5% IACS, 185 MPa, 150 MPa, and 14%, respectively. The conductivity, tensile strength, yield strength, and elongation of the obtained aluminum alloy strip for power supply in new energy vehicles can be 59.5% IACS, 105 MPa, 55 MPa, and 18%, respectively.

[0004] Patent (CN116748326A) discloses a conductive profile of 6101-T63 aluminum alloy and its preparation method and application. The preparation method mainly includes the following steps: melting and casting aluminum rods according to the national standard composition of 6101 aluminum alloy, homogenization treatment, preheating the casting rod and extrusion die, extrusion, solution treatment, and artificial aging treatment. The wall thickness of the conductive profile after forming is not greater than 8mm, and its conductivity is ≥56%IACS, tensile strength is ≥185MPa, yield strength is ≥150MPa, straightness is ≤0.5mm / m, and cross-sectional profile is ≤0.2mm.

[0005] Patent (CN117587306A) discloses a 6101 aluminum alloy sheet with improved strength and conductivity, and its preparation method. The composition, by mass percentage, is: 0.46~0.57% Mg, 0.39~0.42% Si, 0.06~0.36% Fe, 0.07% La, 0.13% Ce, Cu≤0.1%, Mn≤0.03%, Cr≤0.03%, unavoidable impurities not exceeding 0.1%, and the balance being Al. The preparation method mainly includes steps such as preparing aluminum alloy ingots, homogenization treatment, and rolling deformation. Before refining the 6101 aluminum alloy melt, a mixed rare earth element containing La and Ce is added to the alloy. Subsequently, the alloy ingot undergoes homogenization treatment and rolling deformation treatment. The tensile strength of the prepared alloy is 177.3MPa~201.8MPa, but the electrical conductivity is only 42.5%IACS~43.99%IACS.

[0006] Patents (CN108546850A and CN116356184A) disclose a method for producing high-conductivity 6101 aluminum alloy sheet and a method for preparing automotive 6101 aluminum alloy sheet, respectively, along with their applications. Both methods involve casting aluminum alloy ingots using the national standard composition of 6101 aluminum alloy, reducing the content of impurity elements and retaining necessary strengthening elements in specific proportions, optimizing the ratio of Si, Fe, and Mg elements, and then employing appropriate sheet rolling and heat treatment processes. Specifically, the sheet prepared by patent (CN108546850A) has an electrical conductivity of 59.75% IACS, a tensile strength of 116 MPa, a yield strength of 85 MPa, and an elongation of 29%. The sheet prepared by patent (CN116356184A) has an electrical conductivity ≥56%, a tensile strength ≥185 MPa, and a yield strength of 155~175 MPa.

[0007] Patent (CN111850350A) discloses an aluminum alloy material for fuses in new energy vehicles and its preparation method. By mass percentage, the alloy composition is: magnesium 0.4-0.75%, silicon 0.4-0.75%, iron 0.05-0.5%, copper 0.05-0.2%, zinc 0.05-0.2%, manganese 0.01-0.1%, chromium 0.01-0.1%, boron 0.04-0.1%, and mixed rare earth elements 0.03-0.15%, with the balance being aluminum. This method, by adding mixed rare earth elements to 6101 aluminum alloy raw materials, results in a tensile strength of approximately 195 MPa and an electrical conductivity of approximately 56% IACS.

[0008] Patent (CN117265348A) discloses a medium-strength, high-conductivity aluminum alloy sheet and its preparation method. The alloy composition, by mass percentage, is: 0.45~0.53% Mg, 0.4~0.46% Si, 0.1~0.5% Cu, Fe ≤ 0.16%, Zn ≤ 0.01%, Mn ≤ 0.03%, Cr ≤ 0.02%, with the balance being impurities and Al. The preparation method mainly includes aluminum alloy ingot preparation, heat treatment, rolling, and solution aging treatment. By adding an appropriate amount of Cu to the standard composition of 6101 aluminum alloy, the prepared aluminum alloy sheet exhibits an electrical conductivity above 53% IACS, a tensile strength higher than 187 MPa, and a hardness greater than 71 HV.

[0009] In addition, the paper (Zhang Ruifeng, Dong Yaguang, Tan Rui, Zhao Hongliang. Influence of mixed rare earth elements on the as-cast microstructure of 6101 aluminum alloy for overhead conductors, Henan Science and Technology Innovation Driven, 2016.09) reported that the average grain size of the as-cast microstructure with 0.2% mixed rare earth elements was 37.02 micrometers, which was reduced by 39.6% compared with the unadded microstructure. The paper (Peng Xiaolan, Wang Hongcheng. Study on performance optimization of Al-Mg-Si aluminum alloy for heat sinks, Journal of Dongguan University of Technology, 2015,22(3):7-11) reported that adding appropriate amounts of B and Gd elements to 6101 aluminum alloy can improve the mechanical, electrical and thermal properties of 6101 aluminum alloy. Furthermore, the dissertation (Huang Jiajun, Research on Composition Improvement and Performance Balance Optimization of 6101 Alloy for Metro Conductive Rails, South China University of Technology, 2022.4) investigated the effects of elements such as Ni, Ce, Cu, and Zn on the microstructure and properties of 6101 aluminum alloy. The results showed that Cu and Zn can promote age hardening of the alloy, but the conductivity decreases with increasing content; the rare earth element Ce can improve the conductivity of the alloy, but significantly reduces its mechanical properties; Ni is the best element for improving the microstructure and achieving performance balance optimization of 6101 aluminum alloy; after optimizing the alloy composition and heat treatment process, the electrical conductivity and tensile strength of the material are 55.2% IACS and 242.2 MPa, respectively. The dissertation (Liu Zhenxing, Research on Aging Heat Treatment of 6101 Aluminum Alloy, Central South University, 2013.5) studied the effect of precipitate type and characteristics on the conductivity of 6101 aluminum alloy under different aging regimes.

[0010] In summary, each method of preparing 6101 aluminum alloy has its advantages and disadvantages. Due to the inverse relationship between strength and conductivity, it is difficult to simultaneously improve both strength and conductivity, resulting in insufficient overall mechanical and electrical properties. Adding appropriate amounts of alloying elements is a relatively simple, clean, and efficient way to synergistically improve the mechanical and electrical properties of aluminum alloys. In particular, the addition of appropriate amounts of rare earth elements can not only purify the aluminum alloy melt and refine the grains, but also have a modifying effect on the second phase and improve the corrosion resistance of the aluminum alloy. However, rare earth elements are more expensive than components such as Al, Mg, and Si in 6101 aluminum alloy, which limits the research, development, production, and application of high-quality rare earth aluminum alloys. With the continuous development of the aluminum industry and the increasing requirements for aluminum alloy performance, preparation costs, and cycle time, there is an urgent need to develop new methods and technologies that improve raw material sourcing and preparation efficiency. Summary of the Invention

[0011] The purpose of this invention is to provide a high-conductivity 6101 aluminum alloy material modified with recycled rare earth and its preparation method, so as to obtain a low-cost, high-conductivity 6101 aluminum alloy material modified with recycled rare earth, thereby meeting the demand for high-conductivity 6101 aluminum alloy materials and low-cost preparation methods in industrial production.

[0012] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A high-conductivity 6101 aluminum alloy material modified with recycled rare earth elements, wherein the aluminum alloy composition by mass percentage includes: 0.03-0.3% recycled rare earth element Sm or La, 0.05-0.1% iron (Fe), and the balance being 6101 aluminum alloy.

[0013] The recycled rare earth modified high conductivity 6101 aluminum alloy material mentioned above uses recycled rare earth elements Sm and La added from rare earth elements Sm and La extracted from rare earth magnetic waste using Mg as a trapping agent to form Mg-Sm master alloy and Mg-La master alloy, respectively. The rare earth magnetic waste is samarium cobalt permanent magnet alloy or lanthanum iron silicon alloy.

[0014] The method for preparing the recycled rare earth modified high conductivity 6101 aluminum alloy material includes the following steps: (1) Prepare alloy raw materials according to the national standard composition requirements for 6101 aluminum alloy; (2) Place the aluminum ingots into the melting furnace and adjust the melt temperature to 740℃~770℃; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain 6101 aluminum alloy melt; (4) The alloy melt temperature is reduced to 690℃~720℃, and part of the magnesium content in 6101 aluminum alloy is added in the form of Al-Mg master alloy; (5) Heat the melt to 740℃~770℃, and introduce refining agent and argon gas into the melt for purification treatment; (6) Adjust the temperature of the aluminum alloy melt to 690℃~720℃, add rare earth elements Sm or La and the remaining Mg in 6101 aluminum alloy in the form of Mg-Sm master alloy or Mg-La master alloy, and stir and keep the alloy melt at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 460℃~490℃ and keep it at that temperature for 8~16 h to homogenize it. (9) Heat the homogenized ingot to 510℃~540℃ and hold for 1~6 h to perform solution quenching; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 175℃~210℃ and kept for 4~18h for aging treatment to obtain high conductivity 6101 aluminum alloy material modified by recycled rare earth.

[0015] The preparation method of the high conductivity 6101 aluminum alloy material modified by recycled rare earth, in step (5), by mass percentage, is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar.

[0016] The method for preparing the recycled rare earth modified high conductivity 6101 aluminum alloy material, in step (6), uses Mg to extract rare earth elements Sm and La from rare earth magnetic waste to prepare Mg-Sm and Mg-La intermediate alloys respectively, including the following steps: The first step involves sequentially cleaning, drying, and crushing the rare earth magnetic waste to obtain rare earth magnetic waste particles with an effective diameter of no more than 5 mm. The second step involves placing rare earth magnetic waste particles in magnesium melt at a temperature of 750~1050℃ under argon protection, keeping it warm and stirring for 10~45 minutes, and then letting the melt stand for 20~60 minutes. The third step is to pour the upper layer of magnesium melt containing rare earth elements into a mold to cool and solidify, forming a Mg-Sm master alloy or a Mg-La master alloy.

[0017] In the preparation method of the high conductivity 6101 aluminum alloy material modified by recycled rare earth, the first step of the crushing process needs to be carried out in an inert gas protective environment, and the diameter of the rare earth magnetic waste particles is 1~3 mm.

[0018] In the preparation method of the high conductivity 6101 aluminum alloy material modified by recycled rare earth, in the second step, the mass ratio of magnesium to rare earth magnetic waste is 0.2~0.8.

[0019] In the preparation method of the high conductivity 6101 aluminum alloy material modified by recycled rare earth, in the second step, the magnesium melt temperature and the holding and stirring time in the preparation process of Mg-Sm master alloy or Mg-La master alloy are 850℃ and 35 min and 950℃ and 25 min, respectively.

[0020] In the preparation method of the high conductivity 6101 aluminum alloy material modified by recycled rare earth, in the third step, the upper layer of magnesium melt containing rare earth elements is poured into a water-cooled iron mold or copper mold and rapidly cooled to obtain a magnesium rare earth master alloy with uniform microstructure distribution.

[0021] In the preparation method of the high conductivity 6101 aluminum alloy material modified by recycled rare earth, in the third step, the content of Sm or La in the prepared Mg-Sm master alloy or Mg-La master alloy is 10%~40% by mass percentage, and the total content of impurity elements Co and Fe is < 0.1%.

[0022] The principle of this invention is as follows: This invention is primarily based on the interaction principles between metal atoms and the selective distribution of the third component in the two phases, enabling rare earth elements in waste samarium-cobalt and lanthanum-iron-silicon magnets to dissolve into another liquid metal. The interaction effect between different element atoms is related to the enthalpy of mixing. A positive enthalpy indicates mutual repulsion and immiscibility between the two elements, while a negative enthalpy indicates mutual attraction and strong affinity. Considering the application of rare earth metals in 6XXX series aluminum alloys, magnesium, a component of 6XXX aluminum alloys, is selected as a scavenger for rare earth elements in samarium-cobalt and lanthanum-iron-silicon magnets. Simultaneously, magnesium is immiscible with other elements in the magnet besides rare earth elements to ensure low impurity element content in the prepared Mg-Sm and Mg-La master alloys. After the rare earth elements in the samarium cobalt and lanthanum iron silicon magnets dissolve into the magnesium melt, they form a magnesium rare earth alloy liquid phase with a relatively low density. After the rare earth elements in the magnets are extracted, the remaining phase is a Co-Fe based alloy with a higher density. The two immiscible phases separate in the crucible, thus obtaining a magnesium rare earth master alloy that can be used for aluminum alloys and a reusable iron cobalt alloy.

[0023] Compared with the inventor's two previously filed Chinese invention patents (CN116751994A and CN117025958A), this invention uses magnesium as the trapping agent, which can be used in aluminum alloys, and the specific implementation scheme and process parameters are different, resulting in different innovations, objectives, and effects. This invention uses magnesium to target and extract rare earth elements Sm and La from samarium-cobalt and lanthanum-iron-silicon alloy waste. The resulting Mg-Sm and Mg-La master alloys have the advantages of low production cost, simple preparation, and significant effects in 6101 aluminum alloys.

[0024] The high conductivity 6101 aluminum alloy of this invention incorporates rare earth elements Sm or La. The improved performance of the alloy is mainly attributed to the following aspects: 1) Refining the α-Al grain size of the matrix: The addition of rare earth elements Sm or La can increase the nucleation rate of the primary α-Al phase, thereby refining the matrix grains and improving the strength and plastic deformation capacity of the material; 2) The addition of rare earth elements Sm or La can reduce the precipitation activation energy, promoting the precipitation of the second phase in the Al matrix and reducing the solid solubility of other elements in the Al matrix. This increases the number density of (Mg,Si) precipitates and AlFeSi precipitates in the alloy, thus achieving precipitation strengthening; on the other hand, the reduced solid solubility of elements such as Mg and Si in the matrix helps to reduce the scattering effect of solid-solid elements on electrons, improving the conductivity of the alloy; 3) The addition of rare earth elements Sm or La helps to modify the iron-rich phase, improving the mechanical and corrosion resistance properties of the aluminum alloy.

[0025] The advantages and beneficial effects of this invention are as follows: This invention adds appropriate amounts of rare earth elements to aluminum alloys, which not only purifies the aluminum alloy melt and refines the grains, but also modifies the second phase and improves the corrosion resistance of the aluminum alloy, resulting in improved quality and efficiency. However, rare earth elements are relatively expensive, increasing production costs. Therefore, this invention not only provides a way to recycle and reuse secondary rare earth metal resources from waste samarium-cobalt and lanthanum-iron-silicon magnets, fully utilizing the role of secondary rare earth metals in aluminum alloys, but also provides a new method for the production of low-cost, high-quality rare earth aluminum alloy materials. The high-conductivity 6101 aluminum alloy material prepared by this invention using recycled rare earth modification exhibits excellent mechanical and electrical properties, with high strength and good electrical conductivity, a tensile strength ≥210 MPa, and an electrical conductivity ≥58% IACS. This invention provides a new method for developing low-cost, high-quality rare earth aluminum alloy materials and for the separation, recycling, and reuse of strategically critical secondary metal resources, with beneficial effects in fields such as new energy vehicles, power, rail transportation, and resource environment. Attached Figure Description

[0026] Figure 1 The image shows the as-cast microstructure of 6101 aluminum alloy modified with 0.05% (mass percentage) recycled rare earth element Sm prepared according to the method in Example 1. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.

[0027] Figure 2 The image shows the as-cast microstructure of 6101 aluminum alloy modified with 0.1% (mass percentage) of recycled rare earth element Sm prepared according to the method in Example 2. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.

[0028] Figure 3 The image shows the as-cast microstructure of 6101 aluminum alloy modified with 0.25% (mass percentage) recycled rare earth element Sm prepared according to the method in Example 3. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.

[0029] Figure 4 The image shows the as-cast microstructure of 6101 aluminum alloy modified with 0.05% (mass percentage) recycled rare earth La prepared according to the method in Example 4. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.

[0030] Figure 5 The image shows the as-cast microstructure of 6101 aluminum alloy modified with 0.1% (mass percentage) recycled rare earth La prepared according to the method in Example 5. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.

[0031] Figure 6The image shows the as-cast microstructure of 6101 aluminum alloy modified with 0.1% (mass percentage) primary rare earth La prepared according to the method of Comparative Example 1. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.

[0032] Figure 7 The image shows the as-cast microstructure of 6101 aluminum alloy without any rare earth modification prepared according to the method of Comparative Example 2. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase. Detailed Implementation

[0033] In its specific implementation, this invention uses recycled rare earth-modified high-conductivity 6101 aluminum alloy material. By mass percentage, the aluminum alloy composition includes: rare earth element Sm or La 0.03~0.3%, iron (Fe) ≤0.1%, and the balance being 6101 aluminum alloy. The added rare earth elements Sm and La are derived from Mg-Sm master alloy and Mg-La master alloy, respectively, formed by extracting rare earth elements Sm and La from rare earth magnetic waste using Mg as a collector. First, rare earth elements Sm and La are extracted from rare earth magnetic waste (Samarium-Cobalt permanent magnet alloy or Lanthanum-Iron-Silicon alloy) using Mg to prepare Mg-Sm and Mg-La master alloys. Second, raw materials are prepared according to the national standard composition of 6101 aluminum alloy, and aluminum ingots are melted. Elements Si, Fe, and Mg are added to the aluminum melt in sequence, and the alloy melt is stirred and kept at a constant temperature. Then, refining agent and argon gas are introduced into the melt for refining. Subsequently, rare earth elements Sm or La are added to the alloy melt as recycled Mg-Sm master alloy or Mg-La master alloy, respectively. After stirring and settling, a homogeneous melt is obtained, which is then cast into ingots. Finally, the ingots are subjected to homogenization, solution quenching, rolling deformation, and aging treatment in sequence to obtain low-cost, high-conductivity 6101 aluminum alloy material modified with recycled rare earth.

[0034] The method for preparing Mg-Sm and Mg-La master alloys by extracting rare earth elements Sm and La from rare earth magnetic waste using Mg element includes the following steps: (1) Rare earth magnetic waste (samarium cobalt permanent magnet alloy or lanthanum iron silicon alloy) is subjected to surface cleaning, drying and crushing treatment in sequence to obtain rare earth magnetic waste particles with an effective diameter of no more than 5 mm. (2) Under argon protection, rare earth magnetic waste particles are placed in magnesium melt at a temperature of 750~1050℃, kept warm and stirred for 10~45 min, and then the melt is allowed to stand for 20~60 min. (3) Pour the upper layer of magnesium melt containing rare earth elements into a mold and cool and solidify to form Mg-Sm master alloy or Mg-La master alloy.

[0035] In step (1) of extracting rare earth elements Sm and La from rare earth magnetic waste to prepare Mg-Sm and Mg-La master alloys respectively, the crushing process should be carried out in an inert gas protection environment, and the diameter of the rare earth magnetic waste particles is preferably 1~3 mm.

[0036] In step (2) of extracting rare earth elements Sm and La from rare earth magnetic waste with Mg to prepare Mg-Sm and Mg-La master alloys respectively, the preferred mass ratio of metallic magnesium to rare earth magnetic waste is 0.2~0.8.

[0037] In step (2) of extracting rare earth elements Sm and La from rare earth magnetic waste with Mg to prepare Mg-Sm and Mg-La master alloys respectively, the preferred magnesium melt temperature and holding and stirring time in the preparation process of Mg-Sm master alloy and Mg-La master alloy are 850℃ and 35 min and 950℃ and 25 min respectively.

[0038] In step (3), rare earth elements Sm and La are extracted from rare earth magnetic waste to prepare Mg-Sm and Mg-La master alloys respectively. The upper layer of magnesium melt containing rare earth elements is poured into a water-cooled iron mold or copper mold and rapidly cooled to obtain a magnesium rare earth master alloy with uniform microstructure distribution.

[0039] In step (3) of extracting rare earth elements Sm and La from rare earth magnetic waste with Mg element to prepare Mg-Sm and Mg-La master alloys respectively, the content of Sm or La in the prepared Mg-Sm master alloy or Mg-La master alloy is 10%~40% by mass percentage, and the total content of impurity elements (such as Co, Fe, etc.) is < 0.1%.

[0040] A method for preparing highly conductive 6101 aluminum alloy material modified with recycled rare earth elements, the method comprising the following steps: (1) Prepare alloy raw materials according to the national standard composition requirements for 6101 aluminum alloy; (2) Place the aluminum ingots into the melting furnace and adjust the melt temperature to 740℃~770℃; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) The alloy melt temperature is reduced to 690℃~720℃, and part of the magnesium content in 6101 aluminum alloy is added in the form of Al-Mg master alloy; (5) Heat the melt to 740℃~770℃, and introduce refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification treatment. (6) Adjust the temperature of the aluminum alloy melt to 690℃~720℃, add rare earth elements Sm or La and the remaining Mg in 6101 aluminum alloy in the form of Mg-Sm master alloy or Mg-La master alloy, stir the alloy melt and keep it at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 460℃~490℃ and keep it at that temperature for 8~16 h to homogenize it. (9) Heat the homogenized ingot to 510℃~540℃ and hold for 1~6 h to perform solution quenching; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 175℃~210℃ and kept for 4~18h for aging treatment to obtain high conductivity 6101 aluminum alloy material modified by recycled rare earth.

[0041] In addition, the salt slag used to prepare Al5Ti1B master alloy by fluoride salt reaction has the following main components and contents: by mass percentage, 60%~90% potassium fluoroaluminate, 0~24% potassium fluoride, 0%~27% aluminum fluoride, and 0~6% magnesium fluoride.

[0042] The present invention will be described in detail below with reference to the accompanying drawings and embodiments, but the scope of protection and application of the present invention is not limited to the following embodiments.

[0043] Example 1

[0044] In this embodiment, the composition of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, by mass percentage, is: 0.05% rare earth element Sm, 0.1% iron Fe, and the balance being 6101 aluminum alloy. By mass percentage, the 6101 aluminum alloy contains: 0.6% magnesium, 0.35% silicon, and the balance Al.

[0045] In this embodiment, the preparation method of the Mg-Sm master alloy includes the following steps: (1) The samarium cobalt permanent magnet alloy waste is cleaned and dried in sequence, and then the samarium cobalt bulk alloy is crushed into particles with a diameter of 1~3 mm under an inert gas protection environment; (2) Prepare the magnesium blocks in a furnace under argon protection according to a mass ratio of 0.6 between magnesium and samarium cobalt permanent magnet alloy particles. Then gradually add the samarium cobalt permanent magnet alloy particles into the magnesium melt, keep it at 850°C and stir for 35 min, and then let it stand for 30 min. (3) Pour the upper layer of magnesium melt containing rare earth elements in the crucible into a water-cooled iron mold for rapid cooling and solidification to obtain Mg-Sm master alloy.

[0046] The prepared Mg-Sm master alloy, by mass percentage, consists of: 27% rare earth element Sm, 0.03% impurity elements Fe and 0.04% Co, with the balance being Mg.

[0047] In this embodiment, the preparation method of highly conductive 6101 aluminum alloy material modified with recycled rare earth element Sm includes the following steps: (1) Prepare raw materials according to the ingredient requirements; (2) Place the aluminum ingots into the melting furnace and adjust the melt temperature to 750°C; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) The temperature of the alloy melt is reduced to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy; (5) Heat the melt to 750°C, and introduce a refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification. (6) Adjust the temperature of the aluminum alloy melt to 720°C, add the rare earth element Sm and the remaining Mg in the form of the Mg-Sm intermediate alloy prepared above, and stir and keep the alloy melt at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 470℃ and hold for 12 h to homogenize it; (9) Heat the homogenized ingot to 530°C and hold for 4 h to perform solution quenching treatment; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 195℃ and held for 12 h for aging treatment to obtain 6101 aluminum alloy material modified with secondary rare earth metal Sm.

[0048] like Figure 1 As shown in the figure, the microstructure of the high conductivity 6101 aluminum alloy material modified by the recycled rare earth element Sm in this embodiment is shown. The tensile strength of the material is 225 MPa and the electrical conductivity is 58.31% IACS.

[0049] Example 2

[0050] In this embodiment, the composition of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, by mass percentage, is: 0.1% rare earth element Sm, 0.1% iron Fe, and the balance being 6101 aluminum alloy. By mass percentage, the 6101 aluminum alloy contains: 0.6% magnesium, 0.35% silicon, and the balance Al.

[0051] In this embodiment, the preparation method of the Mg-Sm master alloy includes the following steps: (1) The samarium cobalt permanent magnet alloy waste is cleaned and dried in sequence, and then the samarium cobalt bulk alloy is crushed into particles with a diameter of 1~3 mm under an inert gas protection environment; (2) Prepare the magnesium blocks in a furnace under argon protection according to a mass ratio of 0.6 between magnesium and samarium cobalt permanent magnet alloy particles. Then gradually add the samarium cobalt permanent magnet alloy particles into the magnesium melt, keep it at 850°C and stir for 35 min, and then let it stand for 30 min. (3) Pour the upper layer of magnesium melt containing rare earth elements in the crucible into a water-cooled iron mold for rapid cooling and solidification to obtain Mg-Sm master alloy.

[0052] The prepared Mg-Sm master alloy, by mass percentage, consists of: 27% rare earth element Sm, 0.02% impurity elements Fe and 0.05% Co, with the balance being Mg.

[0053] In this embodiment, the preparation method of highly conductive 6101 aluminum alloy material modified with recycled rare earth element Sm includes the following steps: (1) Prepare raw materials according to the ingredient requirements; (2) Place the aluminum ingots into the melting furnace and adjust the melt temperature to 750°C; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) The temperature of the alloy melt is reduced to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy; (5) Heat the melt to 750°C, and introduce a refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification. (6) Adjust the temperature of the aluminum alloy melt to 720°C, add the rare earth element Sm and the remaining Mg in the form of the Mg-Sm intermediate alloy prepared above, and stir and keep the alloy melt at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 470℃ and hold for 12 h to homogenize it; (9) Heat the homogenized ingot to 530°C and hold for 4 h to perform solution quenching treatment; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 195℃ and held for 12 h for aging treatment to obtain 6101 aluminum alloy material modified with secondary rare earth metal Sm.

[0054] like Figure 2 As shown, the microstructure of the high-conductivity 6101 aluminum alloy material modified with recycled rare earth element Sm in this embodiment has a tensile strength of 231 MPa and an electrical conductivity of 59.02% IACS. Compared with Example 1, appropriately increasing the amount of Sm added in this embodiment can make the iron-rich phase finer, changing it from needle-like to granular, and can simultaneously increase the material strength and electrical conductivity.

[0055] Example 3

[0056] In this embodiment, the composition of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, by mass percentage, is: 0.25% rare earth element Sm, 0.05% iron Fe, and the balance being 6101 aluminum alloy. By mass percentage, the 6101 aluminum alloy contains: 0.6% magnesium, 0.35% silicon, and the balance Al.

[0057] In this embodiment, the preparation method of the Mg-Sm master alloy includes the following steps: (1) The samarium cobalt permanent magnet alloy waste is cleaned and dried in sequence, and then the samarium cobalt bulk alloy is crushed into particles with a diameter of 1~3 mm under an inert gas protection environment; (2) Prepare the magnesium blocks in a furnace under argon protection according to a mass ratio of 0.6 between magnesium and samarium cobalt permanent magnet alloy particles. Then gradually add the samarium cobalt permanent magnet alloy particles into the magnesium melt, keep it at 850°C and stir for 35 min, and then let it stand for 30 min. (3) Pour the upper layer of magnesium melt containing rare earth elements in the crucible into a water-cooled iron mold for rapid cooling and solidification to obtain Mg-Sm master alloy.

[0058] The prepared Mg-Sm master alloy, by mass percentage, consists of: 27% rare earth element Sm, 0.01% impurity elements Fe and 0.03% Co, with the balance being Mg.

[0059] In this embodiment, the preparation method of highly conductive 6101 aluminum alloy material modified with recycled rare earth element Sm includes the following steps: (1) Prepare raw materials according to the ingredient requirements; (2) Place the aluminum ingots into the melting furnace and adjust the melt temperature to 750°C; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) The temperature of the alloy melt is reduced to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy; (5) Heat the melt to 750°C, and introduce a refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification. (6) Adjust the temperature of the aluminum alloy melt to 720°C, add the rare earth element Sm and the remaining Mg in the form of the Mg-Sm intermediate alloy prepared above, and stir and keep the alloy melt at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 470℃ and hold for 12 h to homogenize it; (9) Heat the homogenized ingot to 530°C and hold for 4 h to perform solution quenching treatment; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 195℃ and held for 12 h for aging treatment to obtain 6101 aluminum alloy material modified with secondary rare earth metal Sm.

[0060] like Figure 3 As shown, the microstructure of the high-conductivity 6101 aluminum alloy material modified with recycled rare earth element Sm in this embodiment has a tensile strength of 214 MPa and an electrical conductivity of 58.11% IACS. Compared with Example 2, this embodiment further increases the amount of Sm added but produces more needle-like iron-rich phases, and the material strength and electrical conductivity decrease slightly.

[0061] Example 4

[0062] In this embodiment, the composition of the recycled rare earth modified high conductivity 6101 aluminum alloy material, by mass percentage, is: rare earth La 0.05%, iron Fe 0.08%, with the balance being 6101 aluminum alloy. By mass percentage, the 6101 aluminum alloy contains: magnesium 0.6%, silicon 0.35%, with the balance being Al.

[0063] In this embodiment, the preparation method of the Mg-La master alloy includes the following steps: (1) The lanthanum-iron-silicon alloy waste is cleaned and dried in sequence, and then the lanthanum-iron-silicon bulk alloy is crushed into particles with a diameter of 1~3 mm under an inert gas protection environment. (2) Prepare the magnesium by mixing the magnesium metal and the lanthanum iron silicon alloy particles at a mass ratio of 0.3. Melt the magnesium block in a heating furnace under argon protection, then gradually add the lanthanum iron silicon alloy particles into the magnesium melt, keep it at 950°C and stir for 35 min, and then let it stand for 30 min. (3) Pour the upper layer of magnesium melt containing rare earth elements in the crucible into a water-cooled iron mold for rapid cooling and solidification to obtain Mg-La master alloy.

[0064] The prepared Mg-La master alloy composition, by mass percentage, is: 21% rare earth element La, 0.04% impurity elements Fe and 0.02% Co, with the balance being Mg.

[0065] In this embodiment, the preparation method of high-conductivity 6101 aluminum alloy material modified with recycled rare earth La includes the following steps: (1) Prepare raw materials according to the ingredient requirements; (2) Place the aluminum ingots into the melting furnace and adjust the melt temperature to 750°C; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) The temperature of the alloy melt is reduced to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy; (5) Heat the melt to 750°C, and introduce a refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification. (6) Adjust the temperature of the aluminum alloy melt to 720°C, add the rare earth element La and the remaining Mg in the form of the Mg-La intermediate alloy prepared above, and stir and keep the alloy melt at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 470℃ and hold for 12 h to homogenize it; (9) Heat the homogenized ingot to 530°C and hold for 4 h to perform solution quenching treatment; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 195℃ and held for 12 h for aging treatment to obtain 6101 aluminum alloy material modified with secondary rare earth metal La.

[0066] like Figure 4 As shown in the figure, the microstructure of the high conductivity 6101 aluminum alloy material modified with recycled rare earth La in this embodiment has a tensile strength of 219 MPa and an electrical conductivity of 58.45% IACS.

[0067] Example 5

[0068] In this embodiment, the composition of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, by mass percentage, is: rare earth La 0.1%, iron Fe 0.06%, with the balance being 6101 aluminum alloy. By mass percentage, the 6101 aluminum alloy contains: magnesium 0.6%, silicon 0.35%, with the balance being Al.

[0069] In this embodiment, the preparation method of the Mg-La master alloy includes the following steps: (1) The lanthanum-iron-silicon alloy waste is cleaned and dried in sequence, and then the lanthanum-iron-silicon bulk alloy is crushed into particles with a diameter of 1~3 mm under an inert gas protection environment. (2) Prepare the magnesium by mixing the magnesium metal and the lanthanum iron silicon alloy particles at a mass ratio of 0.3. Melt the magnesium block in a heating furnace under argon protection, then gradually add the lanthanum iron silicon alloy particles into the magnesium melt, keep it at 950°C and stir for 35 min, and then let it stand for 30 min. (3) Pour the upper layer of magnesium melt containing rare earth elements in the crucible into a water-cooled iron mold for rapid cooling and solidification to obtain Mg-La master alloy.

[0070] The prepared Mg-La master alloy, by mass percentage, consists of: 21% rare earth element La, 0.01% impurity elements Fe and 0.02% Co, with the balance being Mg.

[0071] In this embodiment, the preparation method of high-conductivity 6101 aluminum alloy material modified with recycled rare earth La includes the following steps: (1) Prepare raw materials according to the ingredient requirements; (2) Place the aluminum ingots into the melting furnace and adjust the melt temperature to 750°C; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) The temperature of the alloy melt is reduced to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy; (5) Heat the melt to 750°C, and introduce a refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification. (6) Adjust the temperature of the aluminum alloy melt to 720°C, add the rare earth element La and the remaining Mg in the form of the Mg-La intermediate alloy prepared above, and stir and keep the alloy melt at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 470℃ and hold for 12 h to homogenize it; (9) Heat the homogenized ingot to 530°C and hold for 4 h to perform solution quenching treatment; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 195℃ and held for 12 h for aging treatment to obtain 6101 aluminum alloy material modified with secondary rare earth metal La.

[0072] like Figure 5 As shown, the microstructure of the high-conductivity 6101 aluminum alloy material modified with recycled rare earth La in this embodiment has a tensile strength of 231 MPa and an electrical conductivity of 59.02% IACS. Compared with Example 4, appropriately increasing the amount of La added in this embodiment can make the iron-rich phase finer, changing it from needle-like to granular, and can simultaneously increase the material strength and electrical conductivity.

[0073] Comparative Example 1 In this comparative example, the composition of the high-conductivity 6101 aluminum alloy modified with primary rare earth La by mass percentage is: 0.1% rare earth La, 0.1% iron Fe, and the balance being 6101 aluminum alloy. In the 6101 aluminum alloy by mass percentage, the composition is: 0.6% magnesium, 0.35% silicon, and the balance being Al.

[0074] In this comparative example, the preparation method of 6101 aluminum alloy material includes the following steps: (1) Prepare raw materials according to the composition requirements of 6101 aluminum alloy; (2) Place the aluminum ingots into a melting furnace and adjust the melt temperature to 750°C; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) Lower the alloy melt temperature to 720℃ and add magnesium in the form of Al-Mg master alloy; (5) Heat the melt to 750°C, and introduce a refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification. (6) Adjust the temperature of the aluminum alloy melt to 720°C, add the primary rare earth La into the melt in the form of Al-La master alloy, and stir and keep the alloy melt at a constant temperature to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 470℃ and hold for 12 h to homogenize it. (9) Heat the homogenized ingot to 530°C and hold for 4 h to perform solution quenching treatment; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 195℃ and held for 12 h for aging treatment to obtain 6101 aluminum alloy material modified with native rare earth metal La.

[0075] like Figure 6 As shown, the microstructure of the high-conductivity 6101 aluminum alloy modified with primary rare earth La in this comparative example has a tensile strength of 234 MPa and an electrical conductivity of 59.10% IACS. Compared with Comparative Example 1, Example 5 shows that adding the same amount of recycled rare earth La and primary rare earth La has almost the same effect. Recycled rare earth has lower cost and is more environmentally friendly than primary rare earth.

[0076] Comparative Example 2 In this comparative example, the composition of the high-conductivity 6101 aluminum alloy material without any rare earth modification, by mass percentage, is: 0.1% iron (Fe), with the balance being 6101 aluminum alloy. In the 6101 aluminum alloy, by mass percentage, the composition is: 0.6% magnesium, 0.35% silicon, with the balance being Al.

[0077] In this comparative example, the preparation method of 6101 aluminum alloy material includes the following steps: (1) Prepare raw materials according to the composition requirements of 6101 aluminum alloy; (2) Place the aluminum ingots into a melting furnace and adjust the melt temperature to 750°C; (3) Add silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stir the alloy melt to obtain aluminum alloy melt; (4) Lower the alloy melt temperature to 720℃ and add magnesium in the form of Al-Mg master alloy; (5) Heat the melt to 750°C, and introduce a refining agent (composed of 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B intermediate alloy by fluoride reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar by mass percentage) and argon gas for purification. (6) Adjust the temperature of the aluminum alloy melt to 720℃, keep it at the temperature and let it stand to obtain a uniform alloy melt. (7) Pour the alloy melt into a mold to cool and solidify to obtain an aluminum alloy ingot; (8) Heat the aluminum alloy ingot to 470℃ and hold for 12 h to homogenize it. (9) Heat the homogenized ingot to 530°C and hold for 4 h to perform solution quenching treatment; (10) Rolling deformation treatment is performed on the ingots after solution quenching; (11) The deformed alloy profile is heated to 195℃ and held for 12 h for aging treatment to obtain 6101 aluminum alloy material modified with native rare earth metal La.

[0078] like Figure 7 As shown, the microstructure of the high-conductivity 6101 aluminum alloy material in this comparative example without any rare earth modification is as follows: the tensile strength is 202 MPa, and the electrical conductivity is 57.34% IACS. Compared with Examples 1-5 and Comparative Example 1, Comparative Example 2 shows that adding appropriate amounts of rare earth elements Sm or La to the 6101 aluminum alloy can increase the number density of the iron-rich phase in the alloy, and the morphology transforms into spherical or near-spherical shapes with significantly refined dimensions, thereby simultaneously improving the mechanical and electrical properties of the material.

[0079] The results show that this invention creatively improves the mechanical and electrical properties of 6101 aluminum alloy by adding rare earth elements Sm and La, extracted and recovered from waste samarium-cobalt and lanthanum-iron-silicon magnets, respectively. Furthermore, the alloy melt was refined and purified before adding the rare earth elements, reducing or avoiding the adverse effects of various inclusions / impurities on the rare earth elements. This not only provides a way to recycle and reuse secondary rare earth metal resources from waste samarium-cobalt and lanthanum-iron-silicon magnets, fully utilizing the role of secondary rare earth metals in aluminum alloys, but also provides a method for the production of low-cost, high-quality rare earth aluminum alloy materials. The high-conductivity 6101 aluminum alloy material modified with recycled rare earth elements of this invention exhibits high strength and good electrical conductivity, with a tensile strength ≥210 MPa and an electrical conductivity ≥58% IACS.

Claims

1. A high-conductivity 6101 aluminum alloy material modified by recycled rare earth. It is characterized in that Calculated by mass percentage, the aluminum alloy composition includes components: recycled rare earth element Sm or La 0.03~0.3%, iron Fe 0.05~0.1%, and the balance is 6101 aluminum alloy.

2. The high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 1, It is characterized in that The added recycled rare earth elements Sm and La are respectively derived from Mg-Sm intermediate alloy and Mg-La intermediate alloy formed by extracting rare earth elements Sm and La from rare earth magnetic waste using Mg element as a collector. The rare earth magnetic waste is samarium cobalt permanent magnet alloy or lanthanum iron silicon alloy.

3. A method for preparing the recycled rare earth modified high-conductivity 6101 aluminum alloy material according to claim 1 or 2, It is characterized in that The method comprises the following steps: (1) Prepare alloy raw materials according to the national standard composition requirements of 6101 aluminum alloy; (2) Place the aluminum ingot into a smelting furnace for melting and adjust the melt temperature to 740°C~770°C; (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stirring the alloy melt to obtain a 6101 aluminum alloy melt; (4) The alloy melt temperature is lowered to 690°C~720°C, and part of the magnesium content in the 6101 aluminum alloy is added in the form of Al-Mg master alloy; (5) The melt temperature is heated to 740°C to 770°C, and a refining agent and argon gas are introduced into the melt for purification; (6) The temperature of the aluminum alloy melt is adjusted to 690°C to 720°C, rare earth elements Sm or La and the remaining Mg in the 6101 aluminum alloy are added in the form of Mg-Sm master alloy or Mg-La master alloy, and the alloy melt is stirred and kept at a constant temperature to obtain an alloy melt with uniform composition; (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification; (8) heating the aluminum alloy ingot to 460°C~490°C and keeping it at this temperature for 8~16 h for homogenization treatment; (9) heating the homogenized ingot to 510°C to 540°C and keeping it at that temperature for 1 to 6 hours to perform solution quenching; (10) performing rolling deformation treatment on the ingot after solution quenching treatment; (11) The deformed alloy profile is heated to 175°C~210°C and kept at this temperature for 4~18 hours for aging treatment to obtain a recycled rare earth modified high conductive 6101 aluminum alloy material.

4. The method for preparing the recycled rare earth modified high-conductivity 6101 aluminum alloy material according to claim 3, It is characterized in that In step (5), the composition is 40% sodium cryolite and 46% fluoride salt to prepare Al 5 Ti 1 B master alloy salt slag, 10% aluminum fluoride, 2% calcium fluoride, 2% potassium feldspar.

5. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 3, It is characterized in that In step (6), the rare earth elements Sm and La in the rare earth magnetic waste are extracted with the Mg element to prepare Mg-Sm and Mg-La master alloys respectively, comprising the following steps: The first step is to sequentially clean, dry and crush the rare earth magnetic waste to obtain rare earth magnetic waste particles with an effective diameter of no more than 5 mm; The second step is to place the rare earth magnetic waste particles in a magnesium melt at a temperature of 750-1050°C under argon protection, keep the temperature and stir for 10-45 minutes, and then let the melt stand for 20-60 minutes; The third step is to pour the upper layer of magnesium melt containing rare earth elements into a mold to cool and solidify to form a Mg-Sm master alloy or a Mg-La master alloy.

6. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 5, It is characterized in that In the first step, the crushing process needs to be carried out in an inert gas protection environment, and the diameter of the rare earth magnetic waste particles is 1~3 mm.

7. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 5, It is characterized in that In the second step, the mass ratio of magnesium to rare earth magnetic waste is 0.2~0.

8.

8. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 5, It is characterized in that In the second step, the magnesium melt temperature and the insulation stirring time in the preparation process of the Mg-Sm master alloy or the Mg-La master alloy are 850°C, 35 min and 950°C, 25 min, respectively.

9. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 5, It is characterized in that In the third step, the upper layer of magnesium melt containing rare earth elements is poured into a water-cooled iron mold or copper mold and rapidly cooled to obtain a magnesium-rare earth intermediate alloy with uniform microstructure distribution.

10. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 5, It is characterized in that In the third step, the content of Sm or La in the prepared Mg-Sm master alloy or Mg-La master alloy is 10% to 40% by mass, and the total content of impurity elements Co and Fe is less than 0.1%.

Citation Information

Patent Citations

  • A low-cost 63%iacs high-conductivity duralumin wire and its manufacturing method

    CN105950893B

  • Production method of high-conductivity 6101 aluminum alloy board

    CN108546850A

  • A 6101-T63 temper aluminum alloy coil for battery conductors and its preparation method

    CN110093536B

  • Aluminium alloy material applied for new energy automobile fuse and preparation method thereof

    CN111850350A

  • Production process of high-quality 6101 aluminum alloy coiled strip for new energy automobile power supply