Smelting method of high-manganese and high-aluminum light steel
Through the process flow of electric furnace → LF furnace → VD furnace → LF furnace, combined with the addition of high carbon ferromanganese, electrolytic manganese, carbon powder and the method of adding Al granules in batches, the smelting of high manganese and high aluminum light steel is solved. Problems such as medium Mn steam volatilization, C/Al element floating and reaction explosion have been achieved to achieve stable industrial smelting production of high manganese and high aluminum lightweight steel and uniform composition of finished products.
Patent Information
- Application Number
- CN202410967950.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
AI Technical Summary
In the field of iron and steel metallurgy, it is difficult to achieve stable industrial smelting production of high-manganese and high-aluminum lightweight steel with existing technology, especially due to the volatilization of Mn steam, the difficulty of adding C/Al elements to the surface, and the violent reaction and explosion caused by the addition of large amounts of Al elements. And the problem of homogenization of molten steel with high alloy content.
Adopting the process flow of electric furnace → LF furnace → VD furnace → LF furnace, through the addition of high carbon ferromanganese, electrolytic manganese, carbon powder, etc. in the LF furnace, Al pellets are added in batches and stirred under vacuum conditions, combined with temperature control The amount of alloy added is adjusted to ensure the uniformity of the chemical composition and the achievement of the target composition.
It effectively solves the difficulty of adding C/Al elements, the reaction explosion caused by the large addition of Al elements, and the homogenization of molten steel with high alloy content. It realizes the stable industrial smelting production of high manganese and high aluminum light steel and reduces the cost of steel. Medium gas content.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a method for smelting high-manganese and high-aluminum lightweight steel. Background Art
[0002] For hundreds of years, steel materials have been used to reduce usage and energy consumption by increasing strength and reducing thickness. However, today, the strength of the material has almost reached its limit and there are rigidity constraints. The development of traditional lightweight technology has encountered a bottleneck, and the application and research and development of lightweight steel has also emerged.
[0003] Lightweight steel is mainly achieved by adding lightweight C and Al elements to steel. However, the addition of Al elements will make the material brittle. In order to further increase the amount of Al elements added, Mn elements will be added at the same time to increase the solid solution of Al, thereby reducing the material density to a greater extent. At present, research on lightweight steel mainly focuses on laboratory smelting and alloying of materials, organizational evolution, aging hardening, mechanical properties, corrosion resistance, etc. There are still many problems for industrial smelting, such as the volatilization of Mn vapor during the smelting process, the difficulty of C / Al elements floating up, the violent reaction and explosion caused by the large amount of Al elements added, and the homogenization of molten steel with high alloy content.
[0004] Under the current national strategic needs such as energy conservation and environmental protection, and dual carbon goals, lightweight, high-performance steel material preparation technology will become the development trend of the future industry, and will have a significant impact on the application of lightweight structural steel in my country. Therefore, based on the results of previous tests, a high-manganese, high-aluminum lightweight steel smelting process method is proposed, thereby achieving a breakthrough in the smelting source process and laying the foundation for further lightweight steel full-process production.
[0005] At present, there are few studies on the industrial smelting production of light steel, especially for the smelting of light steel with high C, high Mn and high Al content, the die casting process control method is still immature, and there are many problems, such as the volatilization of Mn vapor in the smelting process, the difficulty of C / Al elements floating up and adding, the violent reaction and explosion caused by the large amount of Al elements added, the homogenization of high alloy content molten steel, etc. The present invention realizes the stable industrial smelting production of high manganese and high aluminum light steel through the method of alloying from electric furnace → LF furnace → VD furnace → LF furnace. Summary of the invention
[0006] The purpose of the present invention is to provide a method for smelting high manganese and high aluminum lightweight steel in view of the above problems.
[0007] The object of the present invention is achieved in this way: a high manganese, high aluminum lightweight steel smelting method, comprising the following steps: step 1: electric furnace smelting: Mn13 and 20Mn23AlV return materials, high carbon ferromanganese, pure iron, electrolytic manganese, lime, lightly burned dolomite and fluorite are added to the electric furnace, the current 39-49KA is supplied for 35-50min, the furnace charge is completely melted, the molten steel temperature reaches 1610-1640℃ for steel tapping, a covering agent is added for heat preservation after steel tapping, and the bottom of the ladle is paved with low carbon lime. The chemical composition mass percentage of the steel tapping is: C: 0.30-0.80%, Si≤0.30%, Mn: 10.00-20.00%, P≤0.030%, S≤0.020%, Cr≤0.30%, Al ≤2.0%, the rest are Fe and inevitable impurities; Step 2: LF furnace refining: the station current is 23-33KA, the molten steel temperature reaches 1610-1650℃, electrolytic manganese, high carbon ferromanganese and carbon powder are added; the current is 23-33KA, strong stirring and mixing, the molten steel temperature out of the station is 1630-1680℃, the chemical composition mass percentage: C: 0.40-1.40%, Si≤0.30%, Mn: 15.50-32.5%, P≤0.030%, S≤0.020%, Cr≤0.30%, Al≤2.0%; the rest are Fe and inevitable impurities; Step 3: VD furnace refining: slag before entering the station, slag thickness ≤50mm, molten steel temperature before treatment 16 20-1660℃, vacuum for 10-20min under vacuum degree less than 150mbar, then add aluminum particles in 3-6 batches, the single addition amount of aluminum particles is controlled at 0.3-0.8t, and argon gas needs to be blown at the bottom of the ladle for stirring for 5-10min after each addition. The chemical composition of the outgoing molten steel is as follows: C: 0.35-1.30%, Si≤0.30%, Mn: 14.00-30.00%, P≤0.030%, S≤0.020%, Cr≤0.30%, Al: 4.5-11.0%; the rest is Fe and unavoidable impurities; Step 4: LF furnace refining: current 23-33KA power supply temperature adjustment, carbon adjustment with carbon powder, aluminum adjustment with aluminum particles, manganese adjustment with electrolytic manganese, Ferrosilicon adjusts silicon, feeds pure calcium wire 2-4m / t steel, sends electricity to heat up to 1480-1550℃, hard blowing time is 8-15 minutes, total flow rate is 150-300L / min, samples are taken for analysis of composition, soft blowing is performed after confirming that the composition is qualified, soft blowing time is 10-20 minutes, total flow rate is 60-140L / min, slag surface shows obvious creeping and molten steel is not exposed, after treatment, mold injection, the temperature of molten steel out of the station is 1460-1530℃, chemical composition quality percentage: C: 0.50%~1.5%, Mn: 15.0%~32.0%, Al: 5.0%~12.0%, Si: 0.10%~3.0%, P≤0.030%, S≤0.020%, Cr≤0.30%; the rest is Fe and unavoidable impurities; Step 5: Mold casting: The steel ingot mold is baked before pouring, the baking temperature is 60-150℃, the pouring method is used for pouring and argon sealing protection, and 1150-1200℃ low melting point protective slag is selected to be added. The addition amount is 1.3-2.3kg / t per steel ingot. The pre-casting temperature is 1420-1510℃, and the pre-casting flow steel is 0.2-0.3 tons. After the steel is poured, the standing time is required to be more than 2 hours. .
[0008] The mass percentage of chemical composition of the Mn13 return material in step one: C: 0.90-1.20%, Si: 0.30-0.80%, Mn: 11.00-14.00%, P≤0.035%, S≤0.030%, Cr: 0.30-1.00%, Al: 0.01-0.03%; the rest are Fe and unavoidable impurities; the mass percentage of chemical composition of the 20Mn23AlV return material: C: 0.12-0.20%, Si≤0.50%, Mn: 21.50-25.00%, P≤0.030%, S≤0.030%, V: 0.02-0.10%, Al: 1.50-2.50%; the rest are Fe and unavoidable impurities.
[0009] The chemical composition weight percentage of high manganese and high aluminum lightweight steel applicable to this method is: C: 0.50% ~ 1.5%, Mn: 15.0% ~ 32.0%, Al: 5.0% ~ 12.0%, Si: 0.10% ~ 3.0%, P ≤ 0.03%, S ≤ 0.02%, Cr ≤ 0.30%, and the balance is Fe and unavoidable impurities.
[0010] The beneficial effects of the present invention are as follows: the electric furnace of the present invention uses high-carbon and high-manganese scrap steel to reduce the amount of Mn and smelting time of the next process LF furnace; the first LF furnace is equipped with high-carbon ferromanganese, electrolytic manganese, carbon powder, etc. to add manganese and carbon to the upper limit of the composition target; Al particles are added in batches in the VD furnace, and stirring is increased to ensure the uniformity of the Al element in the molten steel; the second LF furnace is adjusted by temperature adjustment and appropriate adjustment of the amount of alloy added to ensure that the target chemical composition is hit. The implementation of this process scheme effectively solves the problems of C / Al elements being easy to float and difficult to add, violent reactions and explosions caused by the large amount of Al elements added, and the homogenization of molten steel with high alloy content, and realizes the stable industrial smelting production of high-manganese and high-aluminum lightweight steel. A step-by-step manganese and aluminum alloy addition process method is adopted. Stable smelting production of high-manganese and high-aluminum lightweight steel is realized. A vacuum treatment link is added to reduce the gas content in the steel. DETAILED DESCRIPTION
[0011] The smelting process designed by the present invention is electric furnace → LF furnace → VD furnace → LF furnace. The electric furnace uses high-carbon and high-manganese scrap steel to reduce the amount of Mn and smelting time of the next process LF furnace; the first LF furnace is equipped with high-carbon ferromanganese, electrolytic manganese, carbon powder, etc. to add manganese and carbon to the upper limit of the component target; Al particles are added in batches in the VD furnace, and stirring is increased to ensure the uniformity of Al elements in the molten steel; the second LF furnace is adjusted by temperature adjustment and appropriate amount of alloy addition to ensure that the target chemical composition is hit. The finished gas content can achieve [H] content ≤5ppm, [0] content ≤10ppm, [N] content ≤10ppm.
[0012] 1. Chemical composition: The chemical composition weight percentage is: C: 0.50% ~ 1.5%, Mn: 15.0% ~ 32.0%, Al: 5.0% ~ 12.0%, Si: 0.10% ~ 3.0%, P ≤ 0.03%, S ≤ 0.02%, Cr ≤ 0.30%, the balance is Fe and unavoidable impurities.
[0013] 2. Smelting: (1) Electric furnace: Electric furnace steelmaking, using Mn13, 20Mn23AlV return materials, high carbon ferromanganese, pure iron, electrolytic manganese, etc. Send electricity for smelting, confirm that all the furnace materials are melted, and the steel tapping temperature is 1610-1640℃. The target chemical composition of steel tapping is to adjust the mass fraction of C element to more than 50% of the target composition of the finished product, and the Mn element is dynamically adjusted according to the proportion of high manganese scrap steel that can be put into use. The remaining elements can be controlled within the range. Use a new steel ladle, add a covering agent for insulation after steel tapping, and use low-carbon lime to pave the bottom of the ladle.
[0014] (2) LF furnace: The time from steel tapping to LF furnace entering the station is ≤ 60 minutes. The station is powered on and samples are taken for chemical composition analysis. According to the analysis results, high carbon ferromanganese, electrolytic manganese and carburizer are added to adjust the composition. Steel tapping can only be performed when the molten steel temperature is 1630-1680℃. The chemical composition of the C element in the steel tapping should be more than 70% of the target composition of the finished product, the Mn element should reach the upper limit of the target of the finished product, and the remaining elements should be controlled within the range.
[0015] (3) VD furnace: When the vacuum is less than 150mbra, add aluminum particles, lime and fluorite in batches after 10 minutes of emptying. After each addition, argon gas should be blown at the bottom of the ladle for stirring for 3-8 minutes, and the argon gas flow rate is 180-280L / min. The amount of aluminum particles added should be limited according to the molten steel tapping temperature to prevent the temperature from dropping too quickly. The target chemical composition of the tapping steel, C and Mn elements are not adjusted, and the Al element is adjusted according to the molten steel temperature and the actual amount required. Try to control it according to the target value ≥70%, and the remaining elements can be controlled within the range.
[0016] (4) LF furnace refining: according to the temperature entering the LF furnace, power is supplied, and samples are taken for chemical composition analysis. Adjust the slag condition and add lime and other slag-forming materials. Add high-carbon ferromanganese, aluminum particles, carbon powder and other alloys to adjust the composition to internal control. Feed the pure calcium line, the pure calcium line feed amount is 2-4m / ton of steel, power is supplied for temperature treatment until the liquidus temperature of the target composition is 120-140℃ higher, the hard blowing time is ≥8 minutes, the total flow rate is 150-300NL / min, take samples for composition analysis, and soft blowing is performed after confirming that the composition is qualified. The soft blowing time is ≥10 minutes, the total flow rate is 60-140NL / min, the slag surface shows obvious creeping and the molten steel is not exposed. The liquidus temperature of the target composition at the exit temperature is 100-120℃ higher.
[0017] 3. Mold casting: The steel mold is cleaned and baked before casting, and the baking temperature is 60-150℃. Use the pouring method for casting and argon sealing protection, so that the steel flow does not produce cold steel nodules. Choose low melting point protective slag to add. The pouring method means that the molten steel enters the ingot mold from the bottom through the center pouring pipe and the bottom plate. Multiple ingots can be cast at the same time. The surface quality of the ingot is good, which is suitable for the casting of small and medium-sized ingots.
[0018] The temperature before casting is 80-120℃ higher than the liquidus temperature. The flow steel before casting is ≥0.2 tons. After the steel is poured, the static time is required to be more than 2 hours. Embodiment 1
[0019] The weight percentages of the smelting target chemical composition are: C: 0.8%, Mn: 22.0%, Al: 5.0%, Si: 0.3%, P≤0.020%, S≤0.015%, and the balance is Fe and unavoidable impurities.
[0020] (1) Electric furnace: The electric furnace uses Mn13 and 20Mn23AlV return materials to smelt steel, and adds some high-carbon ferromanganese, pure iron, electrolytic manganese, etc. It is sent to the power smelting, and it is confirmed that all the furnace materials are melted. The molten steel temperature is 1633℃ for steel tapping. A new steel ladle is used, and a covering agent is added for heat preservation after steel tapping. The bottom of the steel ladle is covered with low-carbon lime. The chemical composition of the steel tapping is C: 0.52%, Mn: 11.3%, P: 0.010%, S: 0.006%, Si: 0.21%, Al: 0.16%, Cr: 0.02.
[0021] (2) LF furnace: The time from steel tapping to LF furnace entry is ≤ 60 minutes. According to the temperature of the LF furnace, power is supplied and samples are taken for chemical composition analysis. The slag condition is adjusted, lime and other slag-making materials are added, and Al particles are added for deoxidation. According to the analysis results, high carbon ferromanganese, electrolytic manganese and carburizer are added to adjust the composition. The molten steel temperature is 1662℃. The chemical composition of the steel tapping is C: 0.77%, Mn: 21.7%, P: 0.011%, S: 0.007%, Si: 0.25%, Al: 0.11%.
[0022] (3) VD furnace: At a vacuum of 50 mbar, after evacuating for 10 minutes, aluminum particles, lime and fluorite are added in three batches. After each addition, argon gas is blown at the bottom of the ladle for stirring for 3-8 minutes, and the argon gas flow rate is 180-280 L / min. The chemical composition of the steel is C: 0.73%, Mn: 20.7%, Al: 4.9%, P: 0.012%, S: 0.006%, Si: 0.28%.
[0023] (4) LF furnace: According to the temperature entering the LF furnace, power is supplied, and samples are taken for chemical composition analysis. Add high carbon ferromanganese, aluminum particles and other alloys to adjust the composition to internal control. Feed the pure calcium line, the feed amount of the pure calcium line is 2-4m / ton of steel, power is supplied for temperature treatment to 1510℃, the hard blowing time is ≥8 minutes, the total flow rate is 150-300L / min, sample and analyze the composition, and soft blowing is performed after confirming that the composition is qualified. The soft blowing time is ≥10 minutes, the total flow rate is 60-140L / min, the slag surface shows obvious creeping and the molten steel is not exposed. The outlet temperature is 1505℃. The chemical composition of the steel is C: 0.78%, Mn: 22.3%, Al: 5.7%, P: 0.012%, S: 0.006%, Si: 0.28%.
[0024] (5) Mold casting: The steel mold is cleaned and baked before casting, and the baking temperature is 100℃. The casting method is adopted and argon sealing protection is used. It is better to prevent the steel flow from producing cold steel nodules. Low melting point protective slag is selected for addition. The pre-casting temperature is 1492℃. The pre-casting flow steel is ≥0.2 tons. After the steel is poured, the static time is required to be more than 2 hours. Embodiment 2
[0025] The weight percentage of the smelting target chemical composition is: C: 1.2%, Mn: 28.0%, Al: 10.0%, Si: 1.0%, P≤0.020%, S≤0.015%, and the balance is Fe and unavoidable impurities.
[0026] (1) Electric furnace: Electric furnace steelmaking, using Mn13, 20Mn23AlV return materials, high carbon ferromanganese, pure iron, electrolytic manganese, etc. Send to power smelting, confirm that all the furnace materials are melted, and the molten steel temperature is 1623℃. Use a new steel ladle, add a covering agent to keep warm after steel is tapped, and use low-carbon lime to lay the bottom of the ladle. The chemical composition of the steel is C: 0.80%, Mn: 16.5%, P: 0.015%, S: 0.008%, Si: 0.23%, Al: 0.35%.
[0027] (2) LF furnace: The time from steel tapping to LF furnace entering the station is ≤ 60 minutes. The station is powered on and samples are taken for chemical composition analysis. The slag condition is adjusted and lime and other slag-making materials are added. High carbon ferromanganese, electrolytic manganese and carburizer are added according to the analysis results to adjust the composition. The molten steel temperature is 1645℃. The chemical composition of the steel tapping is C: 0.98%, Mn: 27.8%, P: 0.010%, S: 0.007%, Si: 0.28%, Al: 0.23%.
[0028] (3) VD furnace: At a vacuum degree of 100 mbra, after evacuating for 10 minutes, aluminum particles, lime and fluorite are added in 5 batches. After each addition, argon gas is blown at the bottom of the ladle for stirring for 3-8 minutes, and the argon gas flow rate is 180-280 L / min. The chemical composition of the steel is C: 0.91%, Mn: 25.9%, Al: 7.3%, P: 0.011%, S: 0.005%, Si: 0.30%.
[0029] (4) LF furnace refining: according to the temperature of the LF furnace, power is supplied, and samples are taken for chemical composition analysis. Adjust the slag condition and add lime and other slag-making materials. Add high carbon ferromanganese, aluminum particles and other alloys to adjust the composition to internal control. Feed pure calcium line, the feed amount of pure calcium line is 2-4m / ton steel, power is supplied for temperature treatment to 1489℃, hard blowing time ≥8 minutes, total flow rate 150-300NL / min, sample and analyze the composition, and soft blowing is performed after confirming that the composition is qualified. Soft blowing time ≥10 minutes, total flow rate 60-140NL / min, slag surface shows obvious creeping and molten steel is not exposed. Outlet temperature 1481℃. Chemical composition of steel output C: 1.16%, Mn: 28.4%, Al: 9.78%, P: 0.011%, S: 0.003%, Si: 0.96%.
[0030] (5) Mold casting: The steel mold is cleaned and baked before casting, and the baking temperature is 80°C. Use the pouring method for casting and argon sealing protection, so that the steel flow does not produce cold steel nodules. Choose low melting point protective slag to add.
[0031] The temperature before casting is 1470℃. The flow steel before casting is ≥0.2 tons. After the steel is poured, the static time is required to be more than 2 hours.
[0032] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.
Claims
1. A method for smelting high manganese and high aluminum lightweight steel, characterized in that: The following steps are involved: Step 1: Electric furnace smelting: Mn13 and 20Mn23AlV return materials, high carbon ferromanganese, pure iron, electrolytic manganese, lime, light-burned dolomite and fluorite are added into the electric furnace, and the current is 39-49KA for 35-50min. The charge is completely melted, and the molten steel temperature reaches 1610-1640℃ for tapping. After tapping, a covering agent is added for insulation, and the bottom of the ladle is paved with low-carbon lime. The chemical composition mass percentage of the tapped steel is: C: 0.30-0.80%, Si≤0.30%, Mn: 10.00-20.00%, P≤0.030%, S≤0.020%, Cr≤0.30%, Al≤2.0%, and the rest is Fe and unavoidable impurities; Step 2: LF furnace refining: the incoming current is 23-33KA, the molten steel temperature reaches 1610-1650℃, and electrolytic manganese, high carbon ferromanganese and carbon powder are added; the current is 23-33KA, and the molten steel temperature out of the station is 1630-1680℃. The chemical composition mass percentage is: C: 0.40-1.40%, Si≤0.30%, Mn: 15.50-32.5%, P≤0.030%, S≤0.020%, Cr≤0.30%, Al≤2.0%; the rest is Fe and unavoidable impurities; Step 3: VD furnace refining: slag is removed before entering the station, slag thickness is ≤50mm, molten steel temperature before treatment is 1620-1660℃, vacuum is drawn for 10-20min at a vacuum degree of less than 150mbar, aluminum particles are added in 3-6 batches, and the single addition amount of aluminum particles is controlled at 0.3-0.8t. After each addition, argon gas needs to be blown at the bottom of the ladle for stirring for 5-10min. The chemical composition of the molten steel out of the station is as follows: C: 0.35-1.30%, Si≤0.30%, Mn: 14.00-30.00%, P≤0.030%, S≤0.020%, Cr≤0.30%, Al: 4.5-11.0%; the rest is Fe and unavoidable impurities; Step 4: LF furnace refining: current 23-33KA, power supply temperature adjustment, carbon adjustment with carbon powder, aluminum adjustment with aluminum particles, manganese adjustment with electrolytic manganese, silicon iron adjustment, feed pure calcium wire 2-4m / t steel, power supply temperature treatment to 1480-1550℃, hard blowing time 8-15 minutes, total flow rate 150-300L / min, sample analysis of components, soft blowing after confirming that the components are qualified, soft blowing time 10-20 minutes, total flow rate 60-140L / mi n, the slag surface shows obvious creep and the molten steel is not exposed. After the treatment, the mold is injected, and the temperature of the molten steel out of the station is 1460-1530℃. The chemical composition mass percentage is: C: 0.50%~1.5%, Mn: 15.0%~32.0%, Al: 5.0%~12.0%, Si: 0.10%~3.0%, P≤0.030%, S≤0.020%, Cr≤0.30%; the rest is Fe and unavoidable impurities; Step 5: Mold casting: The steel ingot mold is baked before pouring, the baking temperature is 60-150℃, the pouring method is used for pouring and argon sealing protection, and 1150-1200℃ low melting point protective slag is selected to be added. The addition amount is 1.3-2.3kg / t per steel ingot. The pre-casting temperature is 1420-1510℃, and the pre-casting flow steel is 0.2-0.3 tons. After the steel pouring is completed, the standing time is required to be more than 2 hours.
2. A method for smelting high manganese and high aluminum lightweight steel according to claim 1, characterized in that: The mass percentage of chemical composition of the Mn13 return material in step one: C: 0.90-1.20%, Si: 0.30-0.80%, Mn: 11.00-14.00%, P≤0.035%, S≤0.030%, Cr: 0.30-1.00%, Al: 0.01-0.03%; the rest are Fe and unavoidable impurities; the mass percentage of chemical composition of the 20Mn23AlV return material: C: 0.12-0.20%, Si≤0.50%, Mn: 21.50-25.00%, P≤0.030%, S≤0.030%, V: 0.02-0.10%, Al: 1.50-2.50%; the rest are Fe and unavoidable impurities.
3. A method for smelting high manganese and high aluminum lightweight steel according to claim 1, characterized in that: The chemical composition weight percentage of high manganese and high aluminum lightweight steel applicable to this method is: C: 0.50% ~ 1.5%, Mn: 15.0% ~ 32.0%, Al: 5.0% ~ 12.0%, Si: 0.10% ~ 3.0%, P ≤ 0.03%, S ≤ 0.02%, Cr ≤ 0.30%, and the balance is Fe and unavoidable impurities.