Manufacturing method of alloy sputtering target material

By combining colloidal chemistry and electrospinning technology, the problem of difficulty in removing impurities and oxygen elements in the preparation of existing alloy sputtering targets has been solved, and the preparation of high-purity and dense alloy sputtering targets has been achieved, improving the quality of thin films. Material properties.

CN118756103APending Publication Date: 2024-10-11JIANGSUTOGE OPTOELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410778097.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Among the existing alloy sputtering target preparation methods, powder metallurgy technology requires high-pressure conditions and is difficult to remove impurities and oxygen elements, affecting the density and purity.

Method used

Using a combination of colloidal chemistry, electrospinning technology and powder metallurgy, a dense alloy sputtering target is formed through preparation of colloidal solution, electrospinning, nanofiber treatment, hydrogen reduction and high-temperature sintering.

Benefits of technology

The uniformity, density and high purity of the alloy sputtering target are achieved, the internal stress and oxygen content are reduced, and the performance of the target is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756103A_ABST
    Figure CN118756103A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of an alloy sputtering target material in the field of sputtering target material preparation. The manufacturing method comprises the following steps: preparing a colloidal solution; preparing a spinning fiber stock solution; electrostatic spinning; carrying out post-treatment on the nanofiber yarns; hydrogen reduction; and high-temperature sintering. The diameter and the structure of the fiber can be accurately controlled through the electrostatic spinning technology, the nanofiber with the specific size and shape is obtained, the prepared alloy sputtering target material has uniformity and consistency, the purity of the alloy is improved through two-stage hydrogen reduction, and through high-temperature sintering and homogenizing annealing, the purity of the alloy is improved. The obtained alloy sputtering target material is more compact and uniform; the hydrazine monohydrochloride can be coordinated with ammonium molybdate and titanium nitrate to form a spinning solution, hydrazine ions and hydroxyl ions are generated through dissociation, the conductivity and viscosity of the spinning solution are improved, and nano-scale uniform cellosilk can be formed easily; the hydrazine monohydrochloride is beneficial to reduction of metal elements into low oxidation states, and is beneficial to realization of more uniform element distribution and more compact particle combination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sputtering target material preparation, and in particular relates to a method for manufacturing an alloy sputtering target material. Background Art

[0002] With the rapid development of the electronics industry, the research of thin film science has become more important. The main method for preparing thin film materials is sputtering. The principle of preparing thin film materials by sputtering is to use abnormal glow discharge to generate plasma from rarefied gas. The plasma is accelerated under the action of the electric field and bombards the surface of the cathode target material with high energy in a certain direction, sputtering the particles on the surface of the target material; the sputtered particles are ejected toward the surface of the substrate in a certain direction, forming a thin film on the surface of the substrate. The material of the cathode target is called a sputtering target. Both metal materials and alloy materials can be used as raw materials for preparing sputtering targets, and under appropriate conditions, alloy sputtering targets can be used for sputtering coating to deposit alloy films with precise proportions.

[0003] Studies have shown that adding an appropriate amount of titanium to molybdenum can significantly improve the corrosion resistance, etching rate matching and adhesion of pure molybdenum films on the diffusion barrier layer. Therefore, molybdenum-titanium alloy targets have become a common material for sputtering coating technology. For the preparation of alloy sputtering targets, the particle size uniformity of the material powder, the density of the target material, and the low oxygen content are all important indicators for evaluating alloy sputtering targets. If you want to prepare a film with good performance, the alloy sputtering target used does not need to meet the above requirements. At present, powder metallurgy technology is generally used to prepare alloy targets, but powder metallurgy sintering requires high pressure conditions to achieve high density, and impurities and oxygen elements are difficult to remove, which affects the density of the alloy target. In view of this, it is necessary to propose a new method for manufacturing alloy sputtering targets. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a method for manufacturing an alloy sputtering target, which combines colloid chemistry, electrospinning technology and powder metallurgy technology to improve the performance of the alloy target.

[0005] In order to achieve the above object, the following technical solution is adopted: The present invention provides a method for manufacturing an alloy sputtering target, comprising the following steps:

[0006] S1. preparing a colloidal solution: dissolving ammonium molybdate and titanium nitrate in deionized water to form a solution, adding hydrazine monohydrochloride to the solution to promote hydrolysis and polymerization of metal ions, and adjusting the pH value and temperature with 0.5 mol / L sodium hydroxide solution to react the metal ions in the solution with hydrazine monohydrochloride to form a colloidal solution;

[0007] S2, preparing spinning fiber stock solution: adding polymer spinning solution to the colloidal solution to form a precursor solution for electrospinning;

[0008] S3, electrospinning: the precursor solution is passed through the nozzle and stretched into filaments under the action of a high voltage electric field, and the solvent evaporates during the flight to form nanofiber filaments;

[0009] S4, post-processing of the nanofibers: crushing and grinding the collected nanofibers to form powders, washing the powders three times with ethanol and deionized water to remove residual organic matter and impurities, and then filtering and drying to obtain nanofiber powders;

[0010] S5, hydrogen reduction: performing two-stage hydrogen reduction on the nanofiber powder to obtain alloy powder;

[0011] S6. High-temperature sintering: The alloy powder is pressed into a desired target shape using a mold, and sintered in a nitrogen atmosphere to combine the powder particles to form a dense alloy target. After sintering, homogenization annealing is performed to reduce internal stress to obtain an alloy sputtering target product.

[0012] Furthermore, the mass ratio of the ammonium molybdate, titanium nitrate, deionized water, hydrazine monohydrochloride and polyvinyl alcohol is 50-80:10-50:100-200:15-45:50-150.

[0013] Furthermore, the polymer spinning solution is one of polyvinyl pyrrolidone, polyvinyl alcohol, polyoxyethylene ether, and polyacrylic acid.

[0014] Furthermore, in step S1, the pH value is adjusted to 7-9, and the temperature is adjusted to 60-80°C.

[0015] Furthermore, the conditions for electrospinning in step S3 are: voltage 10-30 kV, spinning time 10-20 min, and receiving distance 10-30 cm.

[0016] Furthermore, the grinding time in step S4 is 5-10 hours.

[0017] Furthermore, the drying temperature of step S4 is 60-80° C. and the drying time is 12-20 hours.

[0018] Furthermore, the conditions of the two-stage hydrogen reduction are: the first stage reduction temperature is 500-600°C, the hydrogen flow rate is 8-12m3 / h, and the time is 8-12h; the second stage reduction temperature is 800-1000°C, the hydrogen flow rate is 10-15m3 / h, and the time is 8-15h.

[0019] Furthermore, in step S6, the nitrogen sintering temperature is 1500-1800° C., the heating rate is 350-450° C. / h, and the holding time is 8-15h.

[0020] Furthermore, in step S6, the homogenization annealing temperature is 1050-1250° C., and the holding time is 5-15 hours.

[0021] The beneficial effects of the present invention are as follows:

[0022] (1) The present invention can accurately control the diameter and structure of the fiber through electrospinning technology, thereby obtaining nanofibers with specific size and shape. The prepared alloy sputtering target has uniformity and consistency. Impurities can be removed through two-stage hydrogen reduction to improve the purity of the alloy. After high-temperature sintering and homogenization annealing, the obtained alloy sputtering target has reduced internal stress and is more dense and uniform.

[0023] (2) In the present invention, hydrazine monohydrochloride is used before preparing the precursor solution. Hydrazine monohydrochloride can be coordinated with ammonium molybdate and titanium nitrate to form a spinning solution, and hydrazine monohydrochloride is dissociated to produce hydrazine ions and hydroxide ions, thereby improving the conductivity and viscosity of the spinning solution. The increased viscosity helps to form a more stable jet flow during the electrospinning process, and the dissociated ions can form a stable charge layer, which helps to maintain the stability of the fiber and reduce breakage, thereby facilitating the formation of nano-scale uniform fiber filaments;

[0024] (3) The nanofiber filaments prepared by the electrospinning technology of the present invention have a very small diameter and a uniform morphology. The introduced hydrazine monohydrochloride has a reducing property, which helps to reduce the metal elements to their lower oxidation states, thereby helping to achieve a more uniform element distribution and tighter particle bonding in the subsequent reduction and sintering process, thereby improving the density of the target material and reducing the oxide content. The oxygen content of the alloy sputtering target product is further reduced by two-stage hydrogen reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A bar graph showing the oxygen content of the target materials of each embodiment and comparative example of a method for manufacturing an alloy sputtering target material of the present invention;

[0026] Figure 2 The relative density bar graph of the target materials of each embodiment and comparative example of the method for manufacturing an alloy sputtering target material of the present invention is shown;

[0027] Figure 3 It is a bar chart of the purity of the target materials of each embodiment and comparative example of a method for manufacturing an alloy sputtering target material of the present invention;

[0028] Figure 4These are cross-sectional surface SEM photographs of Example 4, Comparative Example 1, and Comparative Example 2 of a method for manufacturing an alloy sputtering target of the present invention.

[0029] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0032] Example 1

[0033] A method for manufacturing alloy sputtering target

[0034] The manufacturing method comprises the following steps:

[0035] S1. preparing a colloidal solution: dissolving ammonium molybdate and titanium nitrate in deionized water to form a solution, adding hydrazine monohydrochloride to the solution to promote hydrolysis and polymerization of metal ions, and adjusting the pH value and temperature with 0.5 mol / L sodium hydroxide solution to react the metal ions in the solution with hydrazine monohydrochloride to form a colloidal solution;

[0036] S2, preparing spinning fiber stock solution: adding polymer spinning solution to the colloidal solution to form a precursor solution for electrospinning;

[0037] S3, electrospinning: the precursor solution is passed through the nozzle and stretched into filaments under the action of a high voltage electric field, and the solvent evaporates during the flight to form nanofiber filaments;

[0038] S4, post-processing of the nanofibers: crushing and grinding the collected nanofibers to form powders, washing the powders three times with ethanol and deionized water to remove residual organic matter and impurities, and then filtering and drying to obtain nanofiber powders;

[0039] S5, hydrogen reduction: performing two-stage hydrogen reduction on the nanofiber powder to obtain alloy powder;

[0040] S6. High-temperature sintering: The alloy powder is pressed into a desired target shape using a mold, and sintered in a nitrogen atmosphere to combine the powder particles to form a dense alloy target. After sintering, homogenization annealing is performed to reduce internal stress to obtain an alloy sputtering target product.

[0041] The mass ratio of the ammonium molybdate, titanium nitrate, deionized water, hydrazine monohydrochloride and polyvinyl alcohol is 50:10:100:15:50.

[0042] The polymer spinning solution is polyvinyl pyrrolidone.

[0043] In step S1, the pH value is adjusted to 7 and the temperature is adjusted to 60°C.

[0044] The conditions for electrospinning in step S3 are: voltage 10 kV, spinning time 10 min, and receiving distance 10 cm.

[0045] The grinding time in step S4 is 5 hours.

[0046] The drying temperature of step S4 is 60° C. and the drying time is 12 h.

[0047] The conditions of the two-stage hydrogen reduction are: the first stage reduction temperature is 500°C, the hydrogen flow rate is 8m 3 / h, the time is 8h, the second stage reduction temperature is 800℃, the hydrogen flow rate is 10m 3 / h, time is 8h.

[0048] In step S6, the nitrogen sintering temperature is 1500° C., the heating rate is 350° C. / h, and the holding time is 8 hours.

[0049] In the step S6, the homogenization annealing temperature is 1050° C. and the holding time is 5 hours.

[0050] Example 2

[0051] A method for manufacturing alloy sputtering target

[0052] The steps included in the manufacturing method are the same as those in Example 1.

[0053] The mass ratio of the ammonium molybdate, titanium nitrate, deionized water, hydrazine monohydrochloride and polyvinyl alcohol is 80:50:200:45:150.

[0054] The polymer spinning solution is polyvinyl alcohol.

[0055] In step S1, the pH value is adjusted to 9 and the temperature is adjusted to 80°C.

[0056] The conditions for electrospinning in step S3 are: voltage 30 kV, spinning time 20 min, and receiving distance 30 cm.

[0057] The grinding time in step S4 is 10 hours.

[0058] The drying temperature of step S4 is 80° C. and the drying time is 20 h.

[0059] The conditions of the two-stage hydrogen reduction are as follows: the first stage reduction temperature is 600°C, the hydrogen flow rate is 12m 3 / h, the time is 12h, the second stage reduction temperature is 1000℃, the hydrogen flow rate is 15m 3 / h, time is 15h.

[0060] In step S6, the nitrogen sintering temperature is 1800° C., the heating rate is 450° C. / h, and the holding time is 15 h.

[0061] In step S6, the homogenization annealing temperature is 1250° C. and the holding time is 15 hours.

[0062] Example 3

[0063] A method for manufacturing alloy sputtering target

[0064] The steps included in the manufacturing method are the same as those in Example 1.

[0065] The mass ratio of the ammonium molybdate, titanium nitrate, deionized water, hydrazine monohydrochloride and polyvinyl alcohol is 58:25:120:25:85.

[0066] The polymer spinning solution is polyoxyethylene ether.

[0067] In step S1, the pH value is adjusted to 7.5 and the temperature is adjusted to 65°C.

[0068] The conditions for electrospinning in step S3 are: voltage 15 kV, spinning time 10 min, and receiving distance 15 cm.

[0069] The grinding time in step S4 is 5-10 hours.

[0070] The drying temperature of step S4 is 70° C. and the drying time is 15 h.

[0071] The conditions of the two-stage hydrogen reduction are: the first stage reduction temperature is 520°C, the hydrogen flow rate is 8m 3 / h, the time is 8h, the second stage reduction temperature is 850℃, the hydrogen flow rate is 12m 3 / h, time is 12h.

[0072] In step S6, the nitrogen sintering temperature is 1600° C., the heating rate is 4000° C. / h, and the holding time is 12 h.

[0073] In step S6, the homogenization annealing temperature is 1100° C. and the holding time is 8 hours.

[0074] Example 4

[0075] A method for manufacturing alloy sputtering target

[0076] The steps included in the manufacturing method are the same as those in Example 1.

[0077] The mass ratio of the ammonium molybdate, titanium nitrate, deionized water, hydrazine monohydrochloride and polyvinyl alcohol is 72:35:160:30:120.

[0078] The polymer spinning solution is polyacrylic acid.

[0079] In step S1, the pH value is adjusted to 8.5 and the temperature is adjusted to 75°C.

[0080] The conditions for electrospinning in step S3 are: voltage 25 kV, spinning time 15 min, and receiving distance 25 cm.

[0081] The grinding time in step S4 is 8.5 hours.

[0082] The drying temperature of step S4 is 75° C. and the drying time is 15 h.

[0083] The conditions of the two-stage hydrogen reduction are: the first stage reduction temperature is 550°C, the hydrogen flow rate is 12m 3 / h, the time is 10h, the second stage reduction temperature is 900℃, the hydrogen flow rate is 12m 3 / h, time is 12h.

[0084] In step S6, the nitrogen sintering temperature is 1750° C., the heating rate is 450° C. / h, and the holding time is 12 h.

[0085] In step S6, the homogenization annealing temperature is 1150° C. and the holding time is 15 hours.

[0086] Comparative Example 1

[0087] The difference between this comparative example and Example 4 is that the non-reducing ligand compound triethylenediamine is used instead of hydrazine monohydrochloride, and the remaining components, component contents, and preparation process are the same as those of Example 1.

[0088] Comparative Example 2

[0089] In this comparative example, a conventional powder metallurgy method is used to prepare an alloy sputtering target. The remaining components, component contents, and preparation process are the same as those in Example 4. The specific preparation method is as follows:

[0090] Molybdenum powder and titanium powder in the same proportion as in the embodiment are weighed and charged into a ball mill, and mixed to form an alloy powder. The alloy powder is pressed into a desired target shape using a mold, and sintered in a nitrogen atmosphere to combine the powder particles to form a dense alloy target. After sintering, homogenization annealing is performed to reduce internal stress to obtain an alloy sputtering target product.

[0091] Results Analysis

[0092] The oxygen content, relative density and purity of each embodiment and comparative example were tested, and the cross section of the target material was observed: the oxygen content of each embodiment and comparative example was measured by ONH-3000 oxygen, nitrogen and hydrogen analyzer, the relative density of each embodiment and comparative example was measured by the measurement method in GB / T 3850-2015, the purity of each embodiment and comparative example was measured by Agilent 5800 inductively coupled plasma spectrometer, and the cross section of the embodiment and comparative example was observed by J-E98HD1 metallographic microscope. The results are shown in FIG. Figure 1-4 .

[0093] Depend on Figure 1-3 In summary, it can be seen that the preparation method of the present invention makes the target material elements evenly distributed and the particles tightly combined. The present invention improves the density of the target material, reduces the oxygen content of the target material, and thus improves the purity of the target material.

[0094] Depend on Figure 4 It can be seen that the grain structure of Example 4 is uniform and fine, the grain structure of Comparative Example 1 is relatively uniform and slightly flawed, and the grain structure of Comparative Example 2 is coarse and flawed. Therefore, the alloy target prepared by the present invention has fine grains, a compact structure, and higher overall performance. The observation results are consistent with Figure 1-3 The measurement results are consistent.

[0095] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0096] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for manufacturing an alloy sputtering target, characterized in that: The steps include: S1. preparing a colloidal solution: dissolving ammonium molybdate and titanium nitrate in deionized water to form a solution, adding hydrazine monohydrochloride to the solution to promote hydrolysis and polymerization of metal ions, and adjusting the pH value and temperature with 0.5 mol / L sodium hydroxide solution to react the metal ions in the solution with hydrazine monohydrochloride to form a colloidal solution; S2, preparing spinning fiber stock solution: adding polymer spinning solution to the colloidal solution to form a precursor solution for electrospinning; S3, electrospinning: the precursor solution is passed through the nozzle and stretched into filaments under the action of a high voltage electric field, and the solvent evaporates during the flight to form nanofiber filaments; S4, post-processing of the nanofibers: crushing and grinding the collected nanofibers to form powders, washing the powders three times with ethanol and deionized water to remove residual organic matter and impurities, and then filtering and drying to obtain nanofiber powders; S5, hydrogen reduction: performing two-stage hydrogen reduction on the nanofiber powder to obtain alloy powder; S6. High-temperature sintering: The alloy powder is pressed into a desired target shape using a mold, and sintered in a nitrogen atmosphere to combine the powder particles to form a dense alloy target. After sintering, homogenization annealing is performed to reduce internal stress to obtain an alloy sputtering target product.

2. The method for manufacturing an alloy sputtering target according to claim 1, characterized in that: The mass ratio of the ammonium molybdate, titanium nitrate, deionized water, hydrazine monohydrochloride, polyvinyl alcohol and sodium alginate is 50-80:10-50:100-200:15-45:50-150.

3. The method for manufacturing an alloy sputtering target according to claim 2, characterized in that: The polymer spinning solution is one of polyvinyl pyrrolidone, polyvinyl alcohol, polyoxyethylene ether and polyacrylic acid.

4. The method for manufacturing an alloy sputtering target according to claim 3, characterized in that: In step S1, the pH value is adjusted to 7-9 and the temperature is adjusted to 60-80°C.

5. The method for manufacturing an alloy sputtering target according to claim 4, characterized in that: The conditions for electrospinning in step S3 are: voltage 10-30 kV, spinning time 10-20 min, and receiving distance 10-30 cm.

6. The method for manufacturing an alloy sputtering target according to claim 5, characterized in that: The grinding time in step S4 is 5-10 hours.

7. The method for manufacturing an alloy sputtering target according to claim 6, characterized in that: The drying temperature of step S4 is 60-80° C. and the drying time is 12-20 hours.

8. The method for manufacturing an alloy sputtering target according to claim 7, characterized in that: The conditions of the two-stage hydrogen reduction are: the first stage reduction temperature is 500-600°C, the hydrogen flow rate is 8-12m 3 / h, the time is 8-12h, the second stage reduction temperature is 800-1000℃, the hydrogen flow rate is 10-15m 3 / h, time is 8-15h.

9. The method for manufacturing an alloy sputtering target according to claim 8, characterized in that: In step S6, the nitrogen sintering temperature is 1500-1800° C., the heating rate is 350-450° C. / h, and the holding time is 8-15h.

10. The method for manufacturing an alloy sputtering target according to claim 9, characterized in that: In step S6, the homogenization annealing temperature is 1050-1250° C., and the holding time is 5-15 hours.