Preparation method of Fe-based hollow nano box material and application of Fe-based hollow nano box material in electrolyzed water

By introducing nickel into the iron-based catalyst and forming Fe-based hollow nanobox materials, the problems of high cost and poor electrocatalytic performance of precious metal catalysts are solved, and efficient electrocatalytic water oxidation and hydrogen evolution reactions are achieved, with performance comparable to precious metal catalysts. performance and long-term stability.

CN118756183APending Publication Date: 2024-10-11FUJIAN TAIMAI HYDROGEN ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410920791.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, noble metal catalysts such as RuO2 and IrO2 have low natural abundance and high price, which limits their wide application in the field of electrocatalytic water splitting, and iron-based catalysts perform poorly in high-efficiency electrocatalytic oxygen evolution and hydrogen evolution reactions. , difficult to replace.

Method used

By rationally introducing nickel element, nickel-iron double metal hydroxide is prepared, and the Fe-based hollow nanobox material is formed through phosphating treatment to enhance its electrocatalytic activity and stability, and the hollow nanostructure is used to provide fast electron transmission channels and rich activity site.

Benefits of technology

It achieves electrocatalytic water oxidation activity and stability comparable to precious metal catalysts, and exhibits excellent catalytic performance and long-term current density stability in electrolyzed water, reducing the cost and energy barrier of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756183A_ABST
    Figure CN118756183A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a Fe-based hollow nano-box material and application of the Fe-based hollow nano-box material in electrolyzed water, in particular to a Fe (OH) 3 nano-material with a hollow nano-box structure prepared by adopting a template etching method. Through simple ion exchange and low-temperature phosphating treatment, the material can be converted into an efficient electrocatalytic oxygen evolution and hydrogen evolution catalyst material; compared with the prior art, the Fe-based catalyst material with the hollow nanostructure is prepared by combining a simple template etching method with ion exchange and low-temperature phosphating treatment; the unique hollow nano-box structure of the Fe-based material provides a large electrocatalytic active area and rich catalytic active sites for an electrocatalytic water decomposition reaction; the particularity of the hollow nano-box structure is beneficial to improving the performance of the catalyst for hydrogen production through water electrolysis, and an innovative solution is provided for development of the catalyst for hydrogen production through water decomposition in the field of electro-catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrolytic water catalytic materials and relates to a Fe-based hollow nano material and a preparation and application thereof. Background Art

[0002] As a green renewable energy, hydrogen is considered to be a promising alternative to traditional fossil energy. With the in-depth development of solar cells, combining electrochemical water splitting devices with solar devices to produce hydrogen has become an effective way of energy conversion; the water splitting reaction is divided into two half reactions: water oxidation to produce oxygen and water reduction to produce hydrogen. Therefore, the development of efficient water oxidation and water reduction electrocatalysts to reduce the energy barrier of the reaction has become a research focus; the current electrocatalysts with the best performance are based on precious metal oxides, such as RuO2 and IrO2, but their low natural abundance and high price have largely limited their large-scale application; therefore, there is an urgent need to develop non-precious metal-based catalysts that are abundant on the earth to replace the expensive Ir and Ru-based precious metal catalysts; in recent years, as researchers have continuously optimized the performance of non-precious metal-based catalysts, their excellent electrocatalytic activity and broad application prospects have attracted more and more research interest.

[0003] Among them, iron, as a non-precious metal element with abundant reserves in the earth's crust, is environmentally friendly and has rich redox states. It has broad application and development prospects in the field of electrocatalytic water decomposition. However, it is currently difficult to effectively use catalyst materials for efficient electrocatalytic oxygen and hydrogen evolution reactions, which is a problem for water decomposition and hydrogen production technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned defects and provide a method for preparing a Fe-based hollow nano-box material and its application in electrolyzed water.

[0005] The inventors of this application have found that, compared with a single iron-based electrocatalytic material, nickel-iron double hydroxide can significantly enhance its electrocatalytic water oxidation activity due to the synergistic effect between metals. In alkaline solution, the electrocatalytic water oxidation activity of nickel-iron hydroxide materials is comparable to that of ruthenium-iridium-based precious metal catalysts. Therefore, by introducing nickel elements into iron-based catalyst materials through a reasonable regulation strategy, the electrocatalytic water oxidation activity of iron-based catalysts can be effectively improved.

[0006] In addition, among non-precious metal-based electrocatalytic hydrogen evolution materials, transition metal phosphides have a Pt-like d-band electronic structure. Given that the electrocatalytic reaction is a reaction process that occurs at the catalyst surface interface, by regulating the morphology and structure of the catalyst material and increasing the specific surface area of ​​the catalyst material, the catalyst can expose more active sites, thereby enhancing the catalyst's electrocatalytic water decomposition performance.

[0007] In addition, when the catalyst has a nano-sized functional shell and a hollow cavity structure, it can provide a short-path electron transport channel for the reaction, which is conducive to rapid charge transport and material transfer, thereby enhancing the electrocatalytic performance of the catalyst material;

[0008] In addition, through research, it is found that, unlike crystalline materials, amorphous materials have disordered atomic arrangements, metastable structures, and rich defect structures. The above characteristics enable amorphous materials to exhibit excellent catalytic performance in the process of electrocatalytic water decomposition; therefore, the inventors of the present application have studied and developed catalyst materials with hollow nanostructures for efficient electrocatalytic oxygen and hydrogen evolution reactions, which is a major breakthrough in the current water decomposition hydrogen production technology.

[0009] The present invention adopts the following technical solutions:

[0010] A method for preparing a Fe-based hollow nano-box material, characterized in that it comprises the following steps:

[0011] Step 1: dissolve copper sulfate in deionized water to form solution A, dissolve sodium citrate and sodium carbonate in deionized water to form solution B, and dissolve glucose in deionized water to form solution C.

[0012] The solution A, solution B and solution C are stirred and mixed evenly, placed in a water bath for heating and reaction, centrifuged, washed with water and alcohol, and dried in an oven to obtain Cu 2 O cubic block powder.

[0013] Step 2: Prepare Cu in step 1 2 The O cubic powder is added to a mixed solution of ethanol and sodium chloride to form a suspension, and then the ethanol solution containing ferric chloride is added dropwise to the above suspension. After the reaction is completed, it is centrifuged, washed with water and alcohol, and then dried in an oven to obtain Fe(OH) 3 Hollow nanobox material.

[0014] Preferably, in step one, the molar ratio of the copper sulfate, sodium citrate, sodium carbonate and glucose is 1:1.1:1.76:2.2.

[0015] Preferably, in the step 1, the temperature of the heating reaction in the water bath is 80° C. and the time is 1 hour.

[0016] Preferably, in step 2, the concentration of ferric chloride is 5-10 mM and the soaking time is 1 hour.

[0017] Application of Fe-based hollow nano-box material in water electrolysis, the Fe(OH) 3 Hollow nano-box materials are used as electrocatalysts in electrocatalytic water decomposition.

[0018] An application of Fe-based hollow nano-box material in electrolysis of water, taking nickel nitrate and dissolving it in deionized water to form solution D, and Fe(OH) prepared in step 2 3 The hollow nano-box material was immersed in solution D, left to soak for a certain period of time, and then centrifuged, washed and dried to obtain Ni-doped Fe(OH) 3 Hollow nano box material; the Ni-doped Fe(OH) 3 Hollow nanobox materials are used for electrocatalytic water oxidation reaction.

[0019] Preferably, the nickel nitrate concentration is 2 mM and the immersion time is 1 h.

[0020] An application of Fe-based hollow nano-box material in electrolysis of water, phosphating treatment is carried out under the protection of inert gas, and the Fe(OH) obtained in step 2 is taken. 3 The hollow nano-box material and sodium hypophosphite are placed in the downwind and upwind ports of a tubular furnace respectively and calcined to obtain an iron phosphide nano-material with a hollow box structure; the iron phosphide nano-material with a hollow box structure is used for electrocatalytic hydrogen evolution reaction.

[0021] Preferably, the sodium hypophosphite and Fe(OH) 3 The mass ratio of the materials is 8 to 15:1.

[0022] Preferably, the calcination temperature of the phosphating treatment is 350° C., the calcination time is 1.5 h, and the heating rate during the calcination process is 2.5° C. / min.

[0023] Compared with the prior art, the advantages and positive effects of the present invention are:

[0024] (1) The present invention successfully prepares an iron hydroxide material with a hollow nano-box structure by a simple template etching method. After ion exchange and phosphating treatment, the iron hydroxide material can be used as an oxygen evolution and hydrogen evolution electrocatalyst for water electrolysis, respectively. This unique hollow nano-box structure has the advantages of a higher specific surface area, a faster charge transfer rate, and abundant material diffusion channels, thereby exposing more active sites for catalytic reactions and facilitating charge transfer and material transfer.

[0025] (2) The iron-based hollow nano-box catalyst material prepared by the present invention has excellent electrolytic water catalytic activity and stability compared with other existing water splitting electrocatalysts. When a two-electrode system is introduced for the full electrolytic water reaction, in a 1M KOH solution, the iron-based hollow nano-box catalyst material has no obvious current decay at a current density of 10 mA cm-2 during constant potential electrolysis for 10 h, indicating that the catalytic system has high catalytic stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Cu 2 SEM image of O nanocube;

[0027] Figure 2 Fe(OH) 3 TEM image of the hollow nanobox;

[0028] Figure 3 Fe(OH) 3 -TEM image of Ni hollow nanobox;

[0029] Figure 4 TEM image of the iron phosphide hollow nanobox;

[0030] Figure 5 Fe(OH) 3 , Fe(OH) 3 -LSV diagram of Ni materials for OER;

[0031] Figure 6 LSV diagram of iron phosphide hollow nanobox material for HER;

[0032] Figure 7 Fe(OH) 3 -Ni and iron phosphide hollow nanobox materials are assembled into a two-electrode system, and the current density-time curve of electrolysis under constant potential conditions. DETAILED DESCRIPTION

[0033] In order to make the purpose and technical solution of the present invention clearer, the present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0034] Embodiment 1:

[0035] Synthesis of Fe-based hollow nanobox materials

[0036] (1)Cu 2 Preparation of O nanocube materials

[0037] First, prepare 10 mL of 34 mM copper sulfate aqueous solution A; then prepare 10 mL of 37 mM sodium citrate and 60 mM sodium carbonate solution B; then prepare 15 mL of 50 mM glucose solution C; finally, stir and mix solutions A, B and C evenly, place them in a water bath and heat them at 80 ° C for 1 h; after the reaction is completed, centrifuge, wash with water and alcohol, and dry them in a 60 ° C oven to obtain Cu 2 O nanocubic block powder material.

[0038] (2)Fe(OH) 3 Preparation of hollow nanobox materials

[0039] 15 mg Cu prepared in step (1) 2 O powder was added to 40 ml of 40 mM sodium chloride alcohol solution to form a suspension, and then 10 ml of 5 mM ferric chloride alcohol solution was added dropwise to the suspension and soaked for 1 hour. After the reaction was completed, it was centrifuged, washed with water and alcohol, and dried in a 60 ° C oven to obtain Fe(OH) 3 Hollow nanobox material.

[0040] (3)Fe(OH) 3 -Preparation of Ni hollow nano-box materials

[0041] Take 7.3 mg of nickel nitrate and dissolve it in 20 ml of deionized water to form a nickel nitrate solution D with a concentration of 2 mM. Add the Fe(OH) 3 The powder material was dispersed and immersed in the above-prepared solution D, and was allowed to stand and soak for 1 h at room temperature and pressure, and then centrifuged, washed and dried to obtain Ni-doped Fe(OH) 3 Hollow nanobox materials can be used for electrocatalytic water oxidation reactions.

[0042] (4) Preparation of iron phosphide hollow nanobox materials

[0043] Take 10 mg Fe(OH) with hollow nano-box structure obtained in step (2) 3 The powder and 80 mg of sodium hypophosphite were placed at the downwind and upwind ports of the tube furnace, respectively. Then, under the protection of argon atmosphere, calcined at 350°C for 1.5 h with a heating rate of 2.5°C / min. After the phosphating treatment was completed, the iron phosphide nanomaterial with a hollow box structure was obtained after water washing and drying, which can be used for electrocatalytic hydrogen evolution reaction.

[0044] Firstly, the morphology of the prepared materials was characterized. Figure 1 The prepared Cu 2 SEM image of O sample, from which it can be seen that the material shows the morphology of nanocubic blocks; Figure 2 Fe(OH) prepared after etching 3 TEM image of the sample, from which it can be seen that the material exhibits a hollow nanostructure; Figure 3 Fe(OH) 3 -TEM image of the Ni sample. It can be seen from the image that the material still maintains the original hollow nanobox structure after ion exchange treatment; Figure 4 This is a SEM picture of iron phosphide material. It can be seen from the picture that although the surface of the material becomes rough after low-temperature phosphating treatment, it still maintains the original hollow nanostructure.

[0045] Combined with the above morphological characterization analysis, it is proved that the iron-based material with hollow nano-box structure has been successfully prepared. The hollow nanostructure of this material will be conducive to the material transport and charge transfer in the electrocatalytic decomposition of water, while exposing more catalytic active sites.

[0046] Embodiment 2:

[0047] The iron-based hollow nano-box material prepared in Example 1 was used as oxygen evolution and hydrogen evolution catalytic electrodes for water electrolysis testing, and the specific steps were as follows:

[0048] The electrocatalytic performance test was carried out in a standard three-electrode system electrolytic cell, with the working electrode being the iron-based hollow nanobox material in step (1), the counter electrode being a carbon rod, and the reference electrode being a saturated calomel electrode. The electrocatalytic water decomposition activity test was carried out in a 1M KOH solution saturated with Ar gas. The scanning speed during the LSV test was 2 mV s –1 The experimental test temperature is 25±2℃.

[0049] Fe(OH) 3 and Fe(OH) 3 -Ni material LSV water oxidation performance test was carried out in 1M KOH solution. Figure 5 As shown, relative to Fe(OH) 3 Materials, Fe(OH) 3 -Ni material exhibits excellent electrocatalytic water oxidation catalytic performance, and the initial overpotential required to drive the water oxidation reaction is about 240mV. In addition, the electrocatalytic hydrogen evolution performance of iron phosphide hollow nanomaterials was carried out in 1M KOH solution. Figure 6 As shown, the current density of electrocatalytic hydrogen evolution of iron phosphide material is 10 mA cm –2 The required overpotential is only 170 mV, which is comparable to the performance of the best iron phosphide catalyst reported so far.

[0050] Furthermore, the Fe(OH) 3 -Ni and iron phosphide materials were used as oxygen evolution and hydrogen evolution catalysts to assemble a two-electrode full water splitting system, and the electrolytic water stability of the catalytic system was tested using the chronoamperometry method. Figure 7 As shown, at 10mA / cm 2 The catalytic current density did not decay significantly when the electrolysis was carried out for 10 h under the condition of current density. The above electrochemical results show that the prepared iron-based hollow nano-box material has high electrocatalytic water decomposition activity and stability in alkaline solution.

[0051] Embodiment 3:

[0052] Synthesis of Fe-based hollow nanobox materials

[0053] (1)Cu 2 Preparation of O nanocube materials

[0054] First, prepare 10 mL of 34 mM copper sulfate aqueous solution A; then prepare 10 mL of 37 mM sodium citrate and 60 mM sodium carbonate solution B; then prepare 30 mL of 50 mM glucose solution C; finally, stir and mix solutions A, B and C evenly, place them in a water bath and heat them at 80 ° C for 1 h; after the reaction is completed, centrifuge, wash with water and alcohol, and dry them in a 60 ° C oven to obtain Cu 2 O nanocubic block powder material.

[0055] (2)Fe(OH) 3 Preparation of hollow nanobox materials

[0056] 15 mg Cu prepared in step (1) 2 O powder was added to 40 ml of 40 mM sodium chloride alcohol solution to form a suspension, and then 10 ml of 5 mM ferric chloride alcohol solution was added dropwise to the suspension and soaked for 1 hour. After the reaction was completed, it was centrifuged, washed with water and alcohol, and dried in a 60 ° C oven to obtain Fe(OH) 3 Hollow nanobox material.

[0057] (3)Fe(OH) 3 -Preparation of Ni hollow nano-box materials

[0058] Take 7.3 mg of nickel nitrate and dissolve it in 20 ml of deionized water to form a nickel nitrate solution D with a concentration of 2 mM. Add the Fe(OH) 3 The powder material was dispersed and immersed in the above-prepared solution D, and was allowed to stand and soak for 1 h at room temperature and pressure, and then centrifuged, washed and dried to obtain Ni-doped Fe(OH) 3 Hollow nanobox materials can be used for electrocatalytic water oxidation reactions.

[0059] (4) Preparation of iron phosphide hollow nanobox materials

[0060] Take 10 mg Fe(OH) with hollow nano-box structure obtained in step (2) 3 The powder and 80 mg of sodium hypophosphite were placed at the downwind and upwind ports of the tube furnace, respectively. Then, under the protection of argon atmosphere, calcined at 350°C for 1.5 h with a heating rate of 2.5°C / min. After the phosphating treatment was completed, the iron phosphide nanomaterial with a hollow box structure was obtained after water washing and drying, which can be used for electrocatalytic hydrogen evolution reaction.

[0061] Embodiment 4:

[0062] Synthesis of Fe-based hollow nanobox materials

[0063] (1)Cu 2 Preparation of O nanocube materials

[0064] First, prepare 10 mL of 34 mM copper sulfate aqueous solution A; then prepare 10 mL of 37 mM sodium citrate and 60 mM sodium carbonate solution B; then prepare 15 mL of 50 mM glucose solution C; finally, stir and mix solutions A, B and C evenly, place them in a water bath and heat them at 80 ° C for 1 h; after the reaction is completed, centrifuge, wash with water and alcohol, and dry them in a 60 ° C oven to obtain Cu 2 O nanocubic block powder material.

[0065] (2)Fe(OH) 3 Preparation of hollow nanobox materials

[0066] 15 mg Cu prepared in step (1) 2 O powder was added to 40 ml of 40 mM sodium chloride alcohol solution to form a suspension, and then 10 ml of 10 mM ferric chloride alcohol solution was added dropwise to the suspension and soaked for 1 hour. After the reaction was completed, it was centrifuged, washed with water and alcohol, and dried in a 60 ° C oven to obtain Fe(OH) 3 Hollow nanobox material.

[0067] (3)Fe(OH) 3 -Preparation of Ni hollow nano-box materials

[0068] Take 7.3 mg of nickel nitrate and dissolve it in 20 ml of deionized water to form a nickel nitrate solution D with a concentration of 2 mM. Add the Fe(OH) 3 The powder material was dispersed and immersed in the above-prepared solution D, and was allowed to stand and soak for 1 h at room temperature and pressure, and then centrifuged, washed and dried to obtain Ni-doped Fe(OH) 3 Hollow nanobox materials can be used for electrocatalytic water oxidation reactions.

[0069] (4) Preparation of iron phosphide hollow nanobox materials

[0070] Take 10 mg Fe(OH) with hollow nano-box structure obtained in step (2) 3The powder and 80 mg of sodium hypophosphite were placed at the downwind and upwind ports of the tube furnace, respectively. Then, under the protection of argon atmosphere, calcined at 350°C for 1.5 h with a heating rate of 2.5°C / min. After the phosphating treatment was completed, the iron phosphide nanomaterial with a hollow box structure was obtained after water washing and drying, which can be used for electrocatalytic hydrogen evolution reaction.

[0071] Embodiment 5:

[0072] Synthesis of Fe-based hollow nanobox materials

[0073] (1)Cu 2 Preparation of O nanocube materials

[0074] First, prepare 10 mL of 34 mM copper sulfate aqueous solution A; then prepare 10 mL of 37 mM sodium citrate and 60 mM sodium carbonate solution B; then prepare 15 mL of 50 mM glucose solution C; finally, stir and mix solutions A, B and C evenly, place them in a water bath and heat them at 80 ° C for 1 h; after the reaction is completed, centrifuge, wash with water and alcohol, and dry them in a 60 ° C oven to obtain Cu 2 O nanocubic block powder material.

[0075] (2)Fe(OH) 3 Preparation of hollow nanobox materials

[0076] 15 mg Cu prepared in step (1) 2 O powder was added to 40 ml of 40 mM sodium chloride alcohol solution to form a suspension, and then 10 ml of 5 mM ferric chloride alcohol solution was added dropwise to the suspension and soaked for 1 hour. After the reaction was completed, it was centrifuged, washed with water and alcohol, and dried in a 60 ° C oven to obtain Fe(OH) 3 Hollow nanobox material.

[0077] (3)Fe(OH) 3 -Preparation of Ni hollow nano-box materials

[0078] Take 7.3 mg of nickel nitrate and dissolve it in 20 ml of deionized water to form a nickel nitrate solution D with a concentration of 2 mM. Add the Fe(OH) 3 The powder material was dispersed and immersed in the above-prepared solution D, and was allowed to stand and soak for 1 h at room temperature and pressure, and then centrifuged, washed and dried to obtain Ni-doped Fe(OH) 3 Hollow nanobox materials can be used for electrocatalytic water oxidation reactions.

[0079] (4) Preparation of iron phosphide hollow nanobox materials

[0080] Take 10 mg Fe(OH) with hollow nano-box structure obtained in step (2) 3 The powder and 150 mg of sodium hypophosphite were placed at the downwind and upwind ports of the tube furnace, respectively. Then, under the protection of argon atmosphere, calcined at 350 ° C for 1.5 h, with a heating rate of 2.5 ° C / min. After the phosphating treatment was completed, the iron phosphide nanomaterial with a hollow box structure was obtained after water washing and drying, which can be used for electrocatalytic hydrogen evolution reaction.

[0081] like Figure 1 to Figure 7 As shown, the present invention successfully prepared an iron hydroxide material with a hollow nano-box structure by a simple template etching method. After ion exchange and phosphating treatment, it can be used as an oxygen evolution and hydrogen evolution electrocatalyst for water electrolysis. This unique hollow nano-box structure has the advantages of high specific surface area, fast charge transfer rate and abundant material diffusion channels, so that more active sites can be exposed for catalytic reactions, which is beneficial to charge transfer and material transfer. Compared with other existing water decomposition electrocatalysts, the iron-based hollow nano-box catalyst material prepared by the present invention has excellent electrolytic water catalytic activity and stability. When a two-electrode system is introduced for the full water electrolysis reaction, in a 1M KOH solution, the iron-based hollow nano-box catalyst material has excellent electrolytic water catalytic activity and stability. –2 At a current density of 1.34 W / m, no obvious current decay occurred during constant potential electrolysis for 10 h, indicating that the catalytic system has high catalytic stability.

[0082] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention still fall within the protection scope of the present invention.

Claims

1. A method for preparing Fe-based hollow nano-box materials, characterized in that: The following steps are involved: Step 1, dissolving copper sulfate in deionized water to form solution A, dissolving sodium citrate and sodium carbonate in deionized water to form solution B, and dissolving glucose in deionized water to form solution C; The solution A, solution B and solution C are stirred and mixed uniformly, placed in a water bath for heating reaction, centrifuged, washed with water and alcohol, and then dried in an oven to obtain Cu2O cubic powder; Step 2: Add the Cu2O cubic powder prepared in step 1 to a mixed solution of ethanol and sodium chloride to form a suspension, and then add the ethanol solution containing ferric chloride dropwise to the above suspension. After the reaction is completed, centrifuge, wash with water and alcohol, and dry in an oven to obtain Fe(OH)3 hollow nano box material.

2. The method for preparing the Fe-based hollow nano-box material according to claim 1, characterized in that: In the step 1, the molar ratio of the copper sulfate, sodium citrate, sodium carbonate and glucose is 1:1.1:1.76:2.

2.

3. The method for preparing the Fe-based hollow nano-box material according to claim 1, characterized in that: In the step 1, the reaction temperature in the water bath is 80° C. and the time is 1 hour.

4. The method for preparing the Fe-based hollow nano-box material according to claim 1, characterized in that: In the step 2, the concentration of ferric chloride is 5-10 mM and the soaking time is 1 hour.

5. An application of the Fe-based hollow nano-box material according to any one of claims 1 to 4 in electrolysis of water, characterized in that: The Fe(OH)3 hollow nano-box material is used as an electrocatalyst in electrocatalytic water decomposition.

6. An application of the Fe-based hollow nano-box material according to claim 1 in electrolyzed water, characterized in that: Dissolve nickel nitrate in deionized water to form solution D, immerse the Fe(OH)3 hollow nano-box material prepared in step 2 in solution D, let it stand for a certain period of time, then wash it with water by centrifugation and dry it, so as to obtain Fe(OH)3 hollow nano-box material doped with Ni; The Ni-doped Fe(OH)3 hollow nano-box material is used for electrocatalytic water oxidation reaction.

7. The method for preparing the Fe-based hollow nano-box material according to claim 6, characterized in that: The nickel nitrate concentration is 2 mM and the immersion time is 1 h.

8. An application of the Fe-based hollow nano-box material according to claim 1 in electrolyzed water, characterized in that: Carry out phosphating treatment under the protection of inert gas, take the Fe(OH)3 hollow nano box material obtained in step 2 and sodium hypophosphite and place them at the downwind and upwind of the tube furnace respectively, and calcine them to obtain the iron phosphide nano material with a hollow box structure; The iron phosphide nanomaterial with a hollow box structure is used for electrocatalytic hydrogen evolution reaction.

9. The method for preparing the Fe-based hollow nano-box material according to claim 8, characterized in that: The mass ratio of the sodium hypophosphite to the Fe(OH)3 material is 8 to 15:

1.

10. The method for preparing the Fe-based hollow nano-box material according to claim 8, characterized in that: The calcination temperature of the phosphating treatment is 350° C., the calcination time is 1.5 h, and the heating rate during the calcination process is 2.5° C. / min.