Platinum-based high-entropy alloy catalyst as well as preparation method and application thereof
Through the co-precipitation method of nitrogen and phosphorus doped carbon supports with platinum salts and transition metal salts, an excellent and stable platinum-based high-entropy alloy catalyst was prepared, which solved the problems of insufficient activity and stability of existing catalysts and achieved efficient electrocatalysis. Improvement of hydrogen evolution performance and platinum atom utilization.
Patent Information
- Application Number
- CN202410781234.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
AI Technical Summary
The platinum carbon catalyst of existing water electrolysis hydrogen production catalysts has low activity and weak binding force between platinum nanoparticles and carriers, which leads to the attenuation of the activity and stability of the catalyst during the electrochemical reaction, and it is difficult to achieve sufficient control and high-efficiency control of platinum active centers using traditional alloy strategies. Entropy alloy materials are widely used.
The co-precipitation method of nitrogen and phosphorus doped carbon carriers with platinum salts and transition metal salts is used to control the formation of ultra-small multi-component platinum-based high-entropy alloy nanoparticles through a combination of surface confinement and co-precipitation methods to improve the utilization of platinum atoms. and controllability of catalyst size, composition, and loading.
Excellent and stable electrocatalytic hydrogen evolution performance is obtained, the amount of platinum precious metal is reduced, the catalyst cost is reduced, and the durability of the catalyst is maintained under harsh conditions.
Smart Images

Figure CN118756199A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen evolution by electrolysis of water, and in particular to a platinum-based high-entropy alloy catalyst and a preparation method and application thereof. Background Art
[0002] Hydrogen has the characteristics of low weight, high calorific value, clean and environmentally friendly, and is an ideal green energy. The process of using renewable energy to electrochemically decompose water to produce hydrogen is simple, feasible, and pollution-free, so it has attracted widespread attention. The electrolytic water hydrogen production catalyst currently used in industry is a platinum-carbon catalyst, which has low intrinsic activity and weak binding force between platinum nanoparticles and carriers. Nanoparticles are prone to migration and agglomeration during the electrochemical reaction, resulting in the attenuation of catalyst activity and stability. Therefore, it is urgent to develop hydrogen evolution catalytic materials with excellent catalytic activity and stability.
[0003] Alloying platinum with other non-precious metals can regulate the electronic structure of platinum species and achieve the adsorption energy of platinum active center atoms and H* intermediates during hydrogen evolution, thereby optimizing catalytic performance. However, traditional alloy strategies are limited to binary and ternary alloys with few components, so the regulation of platinum electronic structure and optimization of intermediate adsorption energy are limited, making it difficult to achieve maximum optimization of catalytic activity. In addition, platinum-based alloys with few components still cannot avoid the dissolution of non-precious metal elements during the reaction process. When the number of elements increases to five or more, the mixing entropy of the material continues to increase, forming a high-entropy alloy material with a large number of unique binding sites. It can effectively regulate the electronic structure of active metals, d-band centers, and strain effects caused by lattice distortion, which has a positive effect on catalytic activity. At the same time, the hysteresis diffusion effect of high-entropy alloys helps to maintain the material structure and composition, achieving excellent durability under harsh working conditions.
[0004] In recent years, the preparation of high-entropy alloy nanomaterials has made certain progress. For example, the carbon thermal shock method can achieve the preparation of high-entropy alloy nanomaterials with a size of 20 to 50 nm, and the high-temperature sintering method is used to prepare materials with a morphology size greater than 100 nm; the preparation conditions of the above methods are harsh and it is difficult to achieve widespread application. In addition, by reducing the metal loading to about 3%, the preparation of high-entropy alloy nanomaterials with a size less than 20 nm can be achieved, but the low-loaded loaded high-entropy alloy catalyst will increase the thickness of the catalytic layer when used for electrochemical reactions, which is not conducive to the multiphase mass transfer process in the electrochemical reaction. Therefore, at this stage, it is urgent to invent a method for preparing ultra-small platinum-based high-entropy alloy nanomaterials with simple operation, controllable components, size, and loading. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a platinum-based high entropy alloy catalyst and a preparation method and application thereof. The platinum-based high entropy alloy catalyst obtained by the preparation method provided by the present invention has excellent and stable electrocatalytic hydrogen evolution performance.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a platinum-based high entropy alloy catalyst, comprising the following steps:
[0008] 1) mixing phytic acid, urea, anhydrous ethanol and activated carbon, drying and firing to obtain a nitrogen-phosphorus doped carbon carrier;
[0009] 2) mixing the nitrogen and phosphorus doped carbon carrier obtained in step 1) with urea, water, platinum salt and transition metal salt, and reacting the mixture to obtain a reactant;
[0010] 3) drying and calcining the reactant obtained in step 2) to obtain a calcined material;
[0011] 4) dispersing the calcined material obtained in step 3) in an acid reagent and then allowing it to stand to obtain a platinum-based high entropy alloy catalyst.
[0012] Preferably, in step 1), the mass ratio of phytic acid, the mass of urea, the volume of anhydrous ethanol and the mass ratio of activated carbon is 0.94 g:0.156 g:50 mL:2.5 g.
[0013] Preferably, the mixing conditions in step 1) include: mixing time of 2 hours and a rotation speed of 500 rpm;
[0014] The drying temperature is 60°C;
[0015] The firing conditions include: firing under argon protection and at a temperature of 800° C. for 2 hours.
[0016] Preferably, in step 2), the mass ratio of the nitrogen and phosphorus doped carbon support to the mass of urea, the volume of water, the mass of the platinum salt, and the mass ratio of the transition metal salt is 100-836 mg: 212 mg: 50 mL: 6.58-23.66 mg: 18.61-74.32 mg.
[0017] Preferably, the transition metal salt includes any four of iron nitrate, cobalt nitrate, nickel nitrate, copper nitrate, manganese nitrate, zinc nitrate and ammonium molybdate.
[0018] Preferably, the reaction conditions of step 2) include: stirring the reaction at an oil bath temperature of 90° C. for 6 h.
[0019] Preferably, the calcination conditions in step 3) include: temperature of 250° C. and time of 2 h.
[0020] Preferably, the acid reagent in step 4) comprises: 0.5 mol / L sulfuric acid solution or 1 mol / L hydrochloric acid solution;
[0021] The standing time is 5 to 12 hours.
[0022] The present invention also provides a platinum-based high-entropy alloy catalyst prepared by the preparation method described in the above technical solution.
[0023] The present invention also provides the use of the platinum-based high entropy alloy catalyst described in the above technical solution in hydrogen evolution by electrolysis of water.
[0024] The preparation method provided by the present invention is based on the combination of surface confinement and co-precipitation, and utilizes the coordination anchoring effect of nitrogen and phosphorus to evenly disperse the metal salt precursor on the carrier. By controlling the concentration of the metal salt precursor and the precipitant (urea in step 2) as well as the reaction temperature and reaction time, the reaction kinetics of the formation process of ultra-small multi-component platinum-based high-entropy alloy nanoparticles can be more accurately regulated to achieve a highly active and highly stable ultra-small platinum-based high-entropy alloy catalyst with controllable size and component loading.
[0025] Compared with the prior art, the present invention has the following beneficial technical effects:
[0026] (1) The preparation method is simple to operate and can realize the preparation of ultra-small high-entropy alloy catalysts with controllable platinum loading (1-10%).
[0027] (2) The high entropy alloy nanoparticles obtained by the preparation method of the present invention are small and uniform in size. By alloying platinum with four or more transition metals, the utilization rate and reaction activity of platinum atoms can be further improved, the amount of platinum precious metal used can be reduced, and the catalyst cost can be reduced.
[0028] (3) Nitrogen and phosphorus doped carriers are beneficial for providing abundant coordination sites and effectively inhibiting the agglomeration of nanoparticles under high-temperature calcination and harsh reaction conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the embodiments are briefly introduced below.
[0030] Figure 1 TEM image of the supported small-sized platinum-based high-entropy alloy catalyst prepared in Example 1;
[0031] Figure 2 The XRD pattern of the supported small-sized platinum-based high-entropy alloy catalyst prepared in Example 1;
[0032] Figure 3 The LSV diagram of the supported small-sized platinum-based high-entropy alloy catalyst prepared in Example 1;
[0033] Figure 4 The stability test of the supported small-sized platinum-based high entropy alloy catalyst prepared in Example 1 before and after the reaction;
[0034] Figure 5 The XRD pattern of the supported small-sized platinum-based high-entropy alloy catalyst prepared in Example 2;
[0035] Figure 6 This is the TEM image of the supported small-sized platinum-based high-entropy alloy catalyst prepared in Example 2. DETAILED DESCRIPTION
[0036] The present invention provides a method for preparing a platinum-based high entropy alloy catalyst, comprising the following steps:
[0037] 1) mixing phytic acid, urea, anhydrous ethanol and activated carbon, drying and firing to obtain a nitrogen-phosphorus doped carbon carrier;
[0038] 2) mixing the nitrogen and phosphorus doped carbon carrier obtained in step 1) with urea, water, platinum salt and transition metal salt, and reacting the mixture to obtain a reactant;
[0039] 3) drying and calcining the reactant obtained in step 2) to obtain a calcined material;
[0040] 4) dispersing the calcined material obtained in step 3) in an acid reagent and then allowing it to stand to obtain a platinum-based high entropy alloy catalyst.
[0041] The present invention mixes phytic acid, urea, anhydrous ethanol and activated carbon, and then dries and burns them to obtain a nitrogen-phosphorus-doped carbon carrier. In the present invention, the mass of the phytic acid, the mass of the urea, the volume of the anhydrous ethanol and the mass ratio of the activated carbon are preferably 0.94g:0.156g:50mL:2.5g. In the present invention, the phytic acid is a phosphorus source, the urea is a nitrogen source, and the activated carbon is a carbon carrier. In the present invention, the mixing conditions preferably include: a time of 2h and a rotation speed of 500rpm. In the present invention, the drying temperature is preferably 60°C. In the present invention, the firing conditions preferably include: roasting for 2h under argon protection and a temperature of 800°C.
[0042] The present invention mixes the obtained nitrogen-phosphorus-doped carbon carrier with urea, water, platinum salt and transition metal salt and reacts to obtain a reactant. In the present invention, the mass ratio of the nitrogen-phosphorus-doped carbon carrier to the mass of urea, the volume of water, the mass of platinum salt and the mass of transition metal salt is preferably 100-836 mg: 212 mg: 50 mL: 6.58-23.66 mg: 18.61-74.32 mg. In the present invention, the transition metal salt preferably includes any four of iron nitrate, cobalt nitrate, nickel nitrate, copper nitrate, manganese nitrate, zinc nitrate and ammonium molybdate. In the present invention, the platinum salt is preferably potassium chloroplatinite. In the present invention, the reaction conditions preferably include: stirring the reaction at an oil bath temperature of 90°C for 6 hours.
[0043] The present invention calcines the obtained reactants after drying to obtain a calcined material. In the present invention, the calcination conditions preferably include: a temperature of 250° C. and a time of 2 hours.
[0044] The present invention disperses the obtained calcined material in an acid reagent and then allows it to stand to obtain a platinum-based high entropy alloy catalyst. In the present invention, the acid reagent preferably includes: 0.5 mol / L sulfuric acid solution or 1 mol / L hydrochloric acid solution. In the present invention, the standing time is preferably 5 to 12 hours.
[0045] The present invention also provides a platinum-based high-entropy alloy catalyst prepared by the preparation method described in the above technical solution.
[0046] The present invention also provides the use of the platinum-based high entropy alloy catalyst described in the above technical solution in hydrogen evolution by electrolysis of water.
[0047] In order to further illustrate the present invention, the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0048] Example 1
[0049] A method for preparing a platinum-based high entropy alloy catalyst, comprising the following steps:
[0050] Step 1: Weigh 0.94g phytic acid and 0.156g urea and dissolve them in 50mL anhydrous ethanol, add 2.5g activated carbon and stir for 2h at a stirring speed of 500rpm. Place the fully dispersed black slurry in a 60℃ oven to dry. The obtained solid mixture is placed in a tube furnace and calcined at 800℃ for 2h in argon protective gas, and then naturally cooled to obtain a nitrogen-phosphorus doped carbon carrier;
[0051] Step 2: Weigh 212 mg of urea and dissolve it in 50 mL of deionized water, then add 6.58 mg of potassium chloroplatinite, 6.47 mg of ferric nitrate nine hydrate, 4.66 mg of cobalt nitrate hexahydrate, 4.65 mg of nickel nitrate hexahydrate, and 4.73 mg of copper nitrate hexahydrate in sequence, and add 100 mg of nitrogen and phosphorus doped carbon carrier after full dissolution. The mixed black solution is placed in a 90 ° C oil bath and stirred for 6 hours. After natural cooling, wash with deionized water, filter and dry. The obtained solid product is calcined in a reducing atmosphere at 250 ° C for 2 hours. The calcined product is ultrasonically dispersed in 50 mL of 0.5 mol / L sulfuric acid solution, and washed with deionized water and filtered after standing for 12 hours. After drying, a supported small-sized platinum-based high-entropy alloy catalyst is obtained.
[0052] Figure 1 The transmission electron microscope image of the obtained small-sized platinum high entropy alloy catalyst is shown below. The size of the high entropy alloy nanoparticles is between 1 and 3 nm and is evenly distributed on the carbon carrier. The platinum loading in the catalyst is about 3.2%, and the total loading of transition metals is 5.2%. Figure 2 There are no obvious metallic characteristic peaks in the XRD pattern, which further indicates that the high entropy alloy nanoparticles are small in size. Figure 3 This is the LSV curve measured in 0.5M sulfuric acid. It can be seen that 10mA / cm 2 When the hydrogen evolution overpotential is 21mV; at 200mA / cm 2 The overpotential of hydrogen evolution is 68 mV, indicating that the catalyst has efficient acidic hydrogen evolution performance. Figure 4 This is a stability test of the catalyst. It can be seen that after 5000 cycles, the hydrogen evolution performance of the catalyst remains almost unchanged, proving that the catalyst has high stability.
[0053] After the metal was loaded in the above examples, the annealing temperature was adjusted to 500° C. and 700° C., respectively, and the obtained catalysts were marked as HEA-500 and HEA-700, respectively. The above catalysts were subjected to hydrogen evolution tests, and the test results are shown in Table 1.
[0054] Table 1 Comparison of hydrogen evolution performance of catalysts prepared at different annealing temperatures
[0055] Serial number <![CDATA[10mA / cm 2 Time potential (mV)]]> <![CDATA[200mA / cm 2 Time potential (mV)]]> HEA-250 21 68 HEA-500 26 117 HEA-700 28 165
[0056] Example 2
[0057] In step 2 of this embodiment, the amount of metals is adjusted to 17.26 mg potassium chloroplatinite, 16.97 mg iron nitrate nonahydrate, 12.22 mg cobalt nitrate hexahydrate, 12.22 mg nickel nitrate hexahydrate, 12.4 mg copper nitrate hexahydrate, and the amount of urea is 555 mg. The other steps are the same as those in Example 1, and an ultra-small platinum-based high-entropy alloy catalyst with a platinum loading of 4.6% is obtained. Figure 5The XRD graph shows that there is still no obvious metal characteristic peak after increasing the metal loading. Figure 6 Transmission electron microscopy images show that high-entropy alloy nanoparticles are evenly dispersed and have a size between 1 and 3 nm.
[0058] Example 3
[0059] In step 2 of this embodiment, the amount of metal is adjusted to 23.66 mg potassium chloroplatinite, 23.43 mg iron nitrate nonahydrate, 16.88 mg cobalt nitrate hexahydrate, 16.87 mg nickel nitrate hexahydrate, 17.14 mg copper nitrate hexahydrate, and 836 mg urea. The other steps are the same as those in Example 1, and an ultra-small platinum-based high-entropy alloy catalyst with a platinum loading of 7.8% is obtained. The size of the high-entropy alloy nanoparticles is 2 to 5 nm.
[0060] Example 4
[0061] In step 2 of this embodiment, 4.06 mg of manganese nitrate was used to replace the copper nitrate in Example 1, and the other steps were the same as Example 1 to obtain an ultra-small platinum-based high entropy alloy catalyst with a platinum loading of 3.5%. The size of the high entropy alloy nanoparticles was 1 to 3 nm.
[0062] Example 5
[0063] In step 2 of this embodiment, 4.75 mg of zinc nitrate was used to replace the copper nitrate in Example 1, and the other steps were the same as Example 1 to obtain an ultra-small platinum-based high entropy alloy catalyst with a platinum loading of 3.0%. The size of the high entropy alloy nanoparticles was 1 to 3 nm.
[0064] Example 6
[0065] In step 2 of this embodiment, 2.83 mg of ammonium molybdate is used to replace the copper nitrate in embodiment 1, and the other steps are the same as those in embodiment 1, to obtain an ultra-small platinum-based high entropy alloy catalyst with a platinum loading of 3.4%. The size of the high entropy alloy nanoparticles is 1 to 3 nm.
[0066] Example 7
[0067] In step 2 of this embodiment, 4.75 mg zinc nitrate and 4.06 mg manganese nitrate are used to replace nickel nitrate and copper nitrate in embodiment 1, and the other steps are the same as those in embodiment 1 to obtain an ultra-small platinum-based high entropy alloy catalyst with a platinum loading of 3.1%. The size of the high entropy alloy nanoparticles is 1 to 3 nm.
[0068] Example 8
[0069] In step 2 of this embodiment, 4.75 mg of zinc nitrate and 2.83 mg of ammonium molybdate are used to replace nickel nitrate and copper nitrate in Example 1, and the other steps are the same as in Example 1 to obtain an ultra-small platinum-based high entropy alloy catalyst with a platinum loading of 3.2%. The size of the high entropy alloy nanoparticles is 1 to 3 nm.
[0070] Example 9
[0071] In step 2 of this embodiment, 4.75 mg of zinc nitrate is used to replace the nickel nitrate in embodiment 1, and the other steps are the same as those in embodiment 1, to obtain an ultra-small platinum-based high entropy alloy catalyst with a platinum loading of 3.3%. The size of the high entropy alloy nanoparticles is 1 to 3 nm.
[0072] Example 10
[0073] In step 2 of this embodiment, 2.83 mg of ammonium molybdate is used to replace the nickel nitrate in embodiment 1, and the other steps are the same as those in embodiment 1 to obtain an ultra-small platinum-based high entropy alloy catalyst with a platinum loading of 3.2%. The size of the high entropy alloy nanoparticles is 1 to 3 nm.
[0074] Table 1 Example 1-10 Water electrolysis hydrogen production activity test
[0075] Serial number <![CDATA[10mA / cm 2 Time potential (mV)]]> <![CDATA[200mA / cm 2 Time potential (mV)]]> Test solution Example 1 21 68 <![CDATA[0.5MH2SO4]]> Example 2 22 72 <![CDATA[0.5MH2SO4]]> Example 3 24 70 <![CDATA[0.5MH2SO4]]> Example 4 22 71 <![CDATA[0.5MH2SO4]]> Example 5 23 69 <![CDATA[0.5MH2SO4]]> Example 6 25 72 <![CDATA[0.5MH2SO4]]> Example 7 21 75 <![CDATA[0.5MH2SO4]]> Example 8 24 73 <![CDATA[0.5MH2SO4]]> Example 9 26 73 <![CDATA[0.5MH2SO4]]> Example 10 25 71 <![CDATA[0.5MH2SO4]]>
[0076] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a platinum-based high entropy alloy catalyst, characterized in that: The following steps are involved: 1) mixing phytic acid, urea, anhydrous ethanol and activated carbon, drying and firing to obtain a nitrogen-phosphorus doped carbon carrier; 2) mixing the nitrogen and phosphorus doped carbon carrier obtained in step 1) with urea, water, platinum salt and transition metal salt, and reacting the mixture to obtain a reactant; 3) drying and calcining the reactant obtained in step 2) to obtain a calcined material; 4) dispersing the calcined material obtained in step 3) in an acid reagent and then allowing it to stand to obtain a platinum-based high entropy alloy catalyst.
2. The preparation method according to claim 1, characterized in that: In the step 1), the mass ratio of phytic acid, the mass of urea, the volume of anhydrous ethanol and the mass ratio of activated carbon is 0.94 g:0.156 g:50 mL:2.5 g.
3. The preparation method according to claim 1, characterized in that: The mixing conditions in step 1) include: mixing time of 2 hours and a rotation speed of 500 rpm; The drying temperature is 60°C; The firing conditions include: firing under argon protection and at a temperature of 800° C. for 2 hours.
4. The preparation method according to claim 1, characterized in that: In the step 2), the mass ratio of the nitrogen and phosphorus doped carbon support to the mass of urea, the volume of water, the mass of the platinum salt, and the mass ratio of the transition metal salt is 100-836 mg: 212 mg: 50 mL: 6.58-23.66 mg: 18.61-74.32 mg.
5. The preparation method according to claim 1 or 4, characterized in that: The transition metal salt includes any four of iron nitrate, cobalt nitrate, nickel nitrate, copper nitrate, manganese nitrate, zinc nitrate and ammonium molybdate.
6. The preparation method according to claim 1, characterized in that: The reaction conditions of step 2) include: stirring the reaction at an oil bath temperature of 90° C. for 6 hours.
7. The preparation method according to claim 1, characterized in that: The calcination conditions in step 3) include: a temperature of 250° C. and a calcination time of 2 hours.
8. The preparation method according to claim 1, characterized in that: The acid reagent in step 4) includes: 0.5 mol / L sulfuric acid solution or 1 mol / L hydrochloric acid solution; The standing time is 5 to 12 hours.
9. A platinum-based high entropy alloy catalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the platinum-based high entropy alloy catalyst according to claim 9 in hydrogen evolution by water electrolysis.
Citation Information
Cited By
Platinum-nickel alloy catalyst with high activity and high stability, preparation method and application of platinum-nickel alloy catalyst in water electrolysis hydrogen evolution reaction in acid medium
CN122169138A