Electrolytic deplating method for chemical nickel plating of aluminum alloy

By using the anodic electrolytic stripping method during the stripping process of aluminum alloy electroless nickel-plated parts, controlling the sulfuric acid solution and current density, termination voltage and power supply soft-start time, the problem of selective corrosion of the substrate is solved and the effective nickel layer is achieved. Removal and recycling of aluminum alloy parts.

CN118756306APending Publication Date: 2024-10-11AEROSPACE LIFE SUPPORT IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410946735.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing electroless nickel-plated aluminum alloy parts are prone to selective corrosion of the substrate during the stripping process, making it difficult to meet the needs of recycling.

Method used

Adopt the anodic electrolytic stripping method, use 180-240g/L sulfuric acid as the electrolytic stripping solution, control the temperature at 13-26°C, the current density at 4-6A/dm2, the time at 10-30 minutes, and the termination voltage at 8- 14V, the surface area ratio of cathode lead plate and anode aluminum alloy parts is 1:3-6, the power supply soft start time is set to more than 180 seconds, and the power supply is turned off when the voltage rises to prevent excessive corrosion.

Benefits of technology

Effectively remove the nickel layer of aluminum alloy parts while preventing selective corrosion of the substrate, ensuring the integrity and recyclability of aluminum alloy parts during the deplating process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756306A_ABST
    Figure CN118756306A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy chemical nickel-plating electrolytic deplating method, and relates to the field of electroplating. The aluminum alloy chemical nickel plating electrolytic stripping method comprises the following steps that anode electrolytic stripping is conducted on an aluminum alloy part subjected to chemical nickel plating, an electrolytic stripping solution comprises 180-240 g / L sulfuric acid, the electrolytic stripping temperature is controlled to be 13-26 DEG C, the current density is controlled to be 4-6 A / dm < 2 >, and the electrolytic stripping time is controlled to be 10-30 min. According to the aluminum alloy chemical nickel plating and electrolytic deplating method, it can be guaranteed that selective corrosion of an aluminum alloy matrix does not occur while a nickel layer on the surface of an aluminum alloy part is deplated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electroplating, and in particular to a method for electrolytic stripping of chemical nickel plating on aluminum alloy. Background Art

[0002] The chemical nickel plating process of aluminum alloy not only improves the corrosion resistance, wear resistance, weldability and other properties of aluminum alloy parts, but also has good bonding between the plating layer and the aluminum alloy substrate, and the plating layer has a beautiful appearance. In addition, the corrosion resistance of chemical nickel plating is better than that of electroplated nickel layer, and it is better than stainless steel in reducing corrosive media. Its own porosity is also very low, so it is widely used.

[0003] However, no matter it is due to processing reasons or surface treatment process reasons, there will always be more or less unqualified chemical nickel-plated aluminum alloy parts. At the same time, the coating of chemical nickel-plated aluminum alloy parts is damaged after a period of use. These chemical nickel-plated aluminum alloy parts are scrapped and need to be de-plated and re-plated for recycling. However, when using nitric acid method for chemical stripping, not only the time required is long, but also because aluminum is an amphoteric metal and has other alloy components, it is difficult to strip evenly, which can easily cause selective uneven corrosion of the base aluminum alloy, making it difficult to meet the needs of recycling. Summary of the invention

[0004] The purpose of the present application is to provide a method for electrolytic stripping of chemical nickel plating on aluminum alloy, which can ensure that the aluminum alloy substrate does not suffer from selective corrosion while the nickel layer on the surface of the aluminum alloy part is stripped.

[0005] This application is implemented as follows:

[0006] The present application provides an aluminum alloy chemical nickel plating electrolytic stripping method, comprising the following steps: performing anodic electrolytic stripping on an aluminum alloy part with chemical nickel plating, wherein the electrolytic stripping solution comprises 180-240 g / L of sulfuric acid, controlling the electrolytic stripping temperature to be 13-26° C., and controlling the current density to be 4-6 A / dm 2 , control the electrolytic stripping time to 10-30min.

[0007] In some optional embodiments, the surface area ratio of the cathode lead plate and the anode aluminum alloy part is controlled to be 1:3-6.

[0008] In some optional embodiments, the termination voltage of the electrolytic stripping is controlled to be 8-14V.

[0009] In some optional implementation schemes, the power soft-start time of the electrolytic stripping is set to be more than 180 seconds.

[0010] In some optional embodiments, during the electrolytic stripping process, when the voltage increases at a rate of 2 V / min, the power supply is turned off to stop the electrolytic stripping.

[0011] The beneficial effect of the present application is that the electrolytic stripping method of chemical nickel plating on aluminum alloy provided by the present application comprises the following steps: performing anodic electrolytic stripping on the chemical nickel-plated aluminum alloy parts, wherein the electrolytic stripping solution comprises 180-240 g / L of sulfuric acid, controlling the electrolytic stripping temperature to be 13-26°C, and controlling the current density to be 4-6 A / dm 2 , and the electrolytic stripping time is controlled to be 10-30 minutes. The electrolytic stripping method for chemical nickel plating of aluminum alloy provided in the present application can ensure that the aluminum alloy substrate does not selectively corrode while the nickel layer on the surface of the aluminum alloy part is stripped. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0013] Figure 1 The method for electrolytic stripping of chemical nickel plating on aluminum alloy provided in the embodiment of the present application is to electrolytically strip the aluminum alloy parts before the chemical nickel plating layer is removed;

[0014] Figure 2 The power supply setting parameters in the aluminum alloy chemical nickel plating electrolytic stripping method provided in the embodiment of the present application;

[0015] Figure 3 The embodiment of the present application provides an aluminum alloy chemical nickel electrolytic stripping method for electrolytically stripping the chemical nickel plating layer from aluminum alloy parts. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0017] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0018] The characteristics and performance of the aluminum alloy chemical nickel plating electrolytic stripping method of the present application are further described in detail below in conjunction with the embodiments.

[0019] The embodiment of the present application provides an aluminum alloy chemical nickel electrolytic stripping method, comprising the following steps: using an organic solvent to clean the aluminum alloy parts with chemical nickel plating, drying the cleaned aluminum alloy parts with chemical nickel plating, hanging the aluminum alloy parts with chemical nickel plating, electrolytically stripping the chemical nickel plating layer of the aluminum alloy parts with steady current, cleaning the aluminum alloy parts with running cold water, cleaning the aluminum alloy parts with alkaline solution, cleaning the aluminum alloy parts with running warm water, cleaning the aluminum alloy parts with running cold water, polishing, cleaning the aluminum alloy parts with running cold water, and drying and unhanging with water and hot air.

[0020] When the chemical nickel plating layer of the aluminum alloy parts is removed by steady-current anode electrolysis, the aluminum alloy parts with chemical nickel plating are used as anodes, the lead plate is used as cathodes, the electrolytic stripping solution includes 180-240g / L sulfuric acid, the electrolytic stripping temperature is controlled to be 13-26°C, and the current density is controlled to be 4-6A / dm 2 , control the electrolytic stripping time to be 10-30min. Optionally, control the surface area ratio of the cathode lead plate and the anode aluminum alloy part to be 1:3-6. Optionally, control the termination voltage of the electrolytic stripping to be 8-14V. Optionally, set the power soft start time of the electrolytic stripping to be more than 180s. Optionally, during the electrolytic stripping process, when the voltage increases at a rate of 2V / min, turn off the power supply to stop the electrolytic stripping.

[0021] The method for electrolytic stripping of chemical nickel plating on aluminum alloy provided in the embodiment of the present application can quickly strip the chemical nickel plating layer on the aluminum alloy by controlling the appropriate electrolytic stripping temperature, electrolytic current density, surface area ratio of cathode lead plate and anode aluminum alloy parts, electrolytic stripping termination voltage, and voltage increase degree, and accurately grasp the timing of forming a resistive oxide film on the surface after the chemical nickel plating layer is stripped to prevent surface corrosion of the aluminum alloy parts and not cause selective over-corrosion to the aluminum alloy part substrate.

[0022] The termination voltage of the electrolytic stripping is controlled to be less than 14V in the embodiment of the present application because the ordinary anodizing constant-voltage oxidation voltage is 14-20V. 14V almost meets the requirements of the winding resistance of the internal and external power lines of all parts, and can ensure the entry of the internal power lines and clean removal of the coating.

[0023] Example 1

[0024] The present application provides an aluminum alloy chemical nickel electrolytic stripping method, which comprises the following steps: using a common anodized DC power supply to electrolytically strip the chemical nickel layer on the surface of the aluminum alloy protective cap part, the electrolytic stripping solution comprises 220g / L sulfuric acid, and the power panel is set as shown in FIG. Figure 2 , set the power supply to run at a steady current, and use a titanium hanger to clamp the chemically nickel-plated aluminum alloy parts such as Figure 1 As shown, the contact is firm. The titanium hanger has the characteristics of ordinary low-voltage anode electrolysis without occupying current. The surface area of ​​the aluminum alloy part is 0.6dm2 , control current density 4-6A / dm 2 , 8 parts are given a current of 25A, the power soft start time is set to 180s, press the start button to run the power supply, and perform anodic electrolysis to strip the chemical nickel plating layer. The current runs stably and the voltage rises slowly. When the voltage exceeds 8V, it increases rapidly and quickly increases to 8.7V. At this time, the voltage rises at a rate of more than 2V / min. Cut off the power supply to start the trough. The electrolytic stripping time is about 10min. A thin anodized film is formed on the parts out of the trough. The alkali washing tank is stripped and the light is exposed to obtain a naked part with a clean chemical nickel plating layer, uniform and bright parts without corrosion. Figure 3 shown.

[0025] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

Claims

1. A method for electrolytic stripping of chemical nickel plating on aluminum alloy, characterized in that: The following steps are involved: Anodic electrolytic stripping is performed on chemically nickel-plated aluminum alloy parts. The electrolytic stripping solution includes 180-240g / L sulfuric acid. The electrolytic stripping temperature is controlled at 13-26°C and the current density is controlled at 4-6A / dm 2 , control the electrolytic stripping time to 10-30min.

2. The method for electrolytic stripping of chemical nickel plating on aluminum alloy according to claim 1, characterized in that: The surface area ratio of the cathode lead plate and the anode aluminum alloy parts is controlled to be 1:3-6.

3. The method for electrolytic stripping of chemical nickel plating on aluminum alloy according to claim 1, characterized in that: The termination voltage of electrolytic stripping is controlled to be 8-14V.

4. The method for electrolytic stripping of chemical nickel plating on aluminum alloy according to claim 1, characterized in that: Set the power soft start time of electrolytic stripping to more than 180s.

5. The method for electrolytic stripping of chemical nickel plating on aluminum alloy according to claim 1, characterized in that: During the electrolytic stripping process, when the voltage increases at a rate of 2 V / min, the power supply is turned off to stop the electrolytic stripping.