Road SGF ultra-thin anti-skid layer and preparation method thereof
By spraying high-viscosity modified emulsified asphalt on the road surface, then spreading steel slag rubber powder and glass fiber, rolling and bonding, and then spraying a second layer of asphalt to form an SGF ultra-thin anti-slip layer, which solves the problem of harsh construction conditions in the existing technology. It achieves the effect of small layer thickness and stable performance, and improves the anti-skid performance and weather resistance.
Patent Information
- Application Number
- CN202410920920.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
AI Technical Summary
The existing ultra-thin covering technology has high requirements on conditions during the construction process, is prone to quality defects, is difficult to reduce in thickness, and has risks of poor surface flatness and delamination cracking.
The first high-viscosity modified emulsified asphalt is sprayed on the road surface, and then the steel slag rubber powder mixture and glass fiber are spread. After the emulsification is broken, it is rolled and bonded, and then the second high-viscosity modified emulsified asphalt is sprayed to form an extremely thin SGF anti-slip layer. , reduce construction condition requirements and improve performance.
The SGF ultra-thin anti-slip layer with small layer thickness and stable performance is realized. The thickness can be reduced to less than 6mm, which improves weather resistance and self-healing, reduces the risk of delamination cracking, lowers the freezing point, and reduces road corrosion and water Stable disease.
Smart Images

Figure CN118756534A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road construction, and in particular to an SGF ultra-thin anti-skid layer for roads and a preparation method thereof. Background Art
[0002] With the rapid development of high-grade highways in my country, it has gradually entered a new stage of "equal emphasis on construction and maintenance" or even focusing on maintenance. In order to extend the service life of high-grade highways and ensure that the comprehensive PQI index reaches excellence, new preventive maintenance technologies have once again attracted widespread attention from the industry. Preventive maintenance technologies for high-grade pavements are generally divided into sealing layers and overlays. The sealing layers include fog sealing layers, gravel sealing layers, fiber sealing layers, slurry sealing layers, micro-surfacing layers, composite sealing layers, etc.; the overlays include thin overlays, ultra-thin overlays, sealing overlays, etc. Taking the most commonly used ultra-thin overlay as an example, it is generally to apply a layer of asphalt mixture with a thickness of 15 to 30 mm on the road surface. The asphalt mixture is mainly composed of coarse and fine aggregates with a certain gradation, mineral powder and asphalt. During construction, generally a layer of asphalt is sprayed on the road surface first, and then the asphalt mixture is spread on the surface and rolled to solidify (see CN108221540A). Ultra-thin overlays can solve problems such as mild cracks in the road surface, attenuation of anti-skid performance, and micro-rutting, and have great application prospects in road maintenance. In order to improve the various properties of the current ultra-thin overlays, researchers have conducted research from the aspects of aggregate type, aggregate gradation, modified emulsified asphalt, and other additives. For example, CN116145492A adds modified glass fiber to the emulsified asphalt layer and the ultra-thin wear layer mixture, strengthens the tight connection between the emulsified asphalt layer and the ultra-thin wear layer, and reduces the porosity of the ultra-thin wear layer of the road to less than 6%, so that rainwater does not remain inside the road surface, and can effectively improve water stability and have good durability; the optimal paving thickness can be reduced to 2cm, and the thinnest limit can reach 1.5cm. For example, CN114538827A introduces steel slag as aggregate, and uses polymer composite rubber modified asphalt as asphalt, which improves the wear resistance of the ultra-thin overlay and optimizes high and low temperature stability and anti-aging performance.
[0003] The current ultra-thin overlay technology generally has the following disadvantages: 1. Since the surface layer is constructed with asphalt mixture, considering the performance of modified emulsified asphalt itself, it is often necessary to introduce fine aggregates and mineral powders with specific grading, and the modified emulsified asphalt in the mixture is often easy to demulsify and loose (demulsification time ≤ 120s), and the construction conditions are relatively high, otherwise it is easy to fail to compact and produce quality defects. 2. Due to the presence of some fine aggregates and mineral powders in the asphalt mixture, it is difficult to fully compact it in the future, and the surface flatness is poor. 3. During the construction process, a paver with a synchronous paving function is often used for operation, that is, a layer of modified emulsified asphalt is sprayed first, and then the asphalt mixture is quickly paved. In order to give full play to the bonding effect of the first sprayed emulsified asphalt, it is necessary to force it to demulsify, which leads to incomplete evaporation of some water, which has an adverse effect on the adhesion of the road surface. Therefore, the ultra-thin overlay thickness of the traditional process can often only be 1.5cm to 2.5cm, and there is a risk of delamination and peeling after further thinning. In response to the above problems, some researchers have changed the emulsified asphalt mixture to hot asphalt mixture to improve the bonding strength and reduce the thickness of the ultra-thin overlay, but this change means that the construction conditions will become more stringent. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing an SGF ultra-thin anti-skid layer for roads. The preparation method is simple and has low requirements on construction conditions. The obtained SGF ultra-thin anti-skid layer has the advantages of small layer thickness and stable performance.
[0005] Another technical problem to be solved by the present invention is to provide an extremely thin SGF anti-skid layer for roads.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing an SGF ultra-thin anti-skid layer of a road, which comprises:
[0007] Spray the first high-viscosity modified emulsified asphalt on the road surface to form a high-viscosity modified emulsified asphalt layer; wherein the spraying amount is 1 to 1.2 L / m 2 ;
[0008] Before the first high-viscosity modified emulsified asphalt is demulsified, the steel slag rubber powder mixture and glass fiber are spread on the high-viscosity modified emulsified asphalt layer to obtain a first intermediate layer; wherein the steel slag rubber powder mixture is a mixture of single-stage steel slag and rubber powder; the total spreading amount of the steel slag rubber powder mixture and glass fiber is 10-12 kg / m 2 The weight ratio of steel slag to rubber powder in the steel slag-rubber powder mixture is 100:1 to 100:3, and the weight ratio of the steel slag-rubber powder mixture to glass fiber is 100:0.2 to 100:1;
[0009] After the first high-viscosity modified emulsified asphalt is demulsified, a rubber-wheeled roller is used to roll and knead the first intermediate layer and the high-viscosity modified emulsified asphalt layer so that the first intermediate layer and the high-viscosity modified emulsified asphalt layer penetrate and bond with each other to obtain a second intermediate layer;
[0010] The second high-viscosity modified emulsified asphalt is sprayed on the surface of the second intermediate layer to obtain a surface layer; wherein the spraying amount is 0.3-0.5 L / m 2 ;
[0011] After the second high-viscosity modified emulsified asphalt is completely demulsified, it is left to stand for 1 to 2 hours to form strength, and the road SGF ultra-thin anti-skid layer is obtained.
[0012] Wherein, the solid content of the first high-viscosity modified emulsified asphalt is greater than the solid content of the second high-viscosity modified emulsified asphalt.
[0013] As an improvement of the above technical solution, the steel slag is selected from single-stage steel slag with a particle size of 3 to 6 mm or single-stage steel slag with a particle size of 4 to 7 mm; and / or
[0014] The rubber powder is obtained by crushing waste tires, and its maximum particle size is ≤ the aperture of the 80-mesh sieve; and / or
[0015] The length of the glass fiber is 5 to 50 mm.
[0016] As an improvement of the above technical solution, the first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt have an Engla viscosity of 1 to 10s at 25°C, a needle penetration of 40 to 120 (0.1 mm), a softening point of ≥50°C, and an elongation of ≥20cm at 5°C;
[0017] The solid content of the first high-viscosity modified emulsified asphalt is ≥65wt%, and the solid content of the second high-viscosity modified emulsified asphalt is 40-50wt%.
[0018] As an improvement of the above technical solution, the first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt are selected from SBS high-viscosity modified emulsified asphalt, SBR high-viscosity modified emulsified asphalt or SBS, SBR composite high-viscosity modified emulsified asphalt.
[0019] As an improvement of the above technical solution, the steel slag is selected from single-stage steel slag with a diameter of 4 to 7 mm; and / or
[0020] The rubber powder is obtained by crushing waste tires, and its maximum particle size is ≤ the aperture of a 100-mesh sieve; and / or
[0021] The length of the glass fiber is 10 to 20 mm; and / or
[0022] The first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt are SBS and SBR composite high-viscosity modified emulsified asphalt, and the weight ratio of SBS to SBR is 3:2 to 7:4.
[0023] As an improvement of the above technical solution, the preparation method of the steel slag rubber powder mixture is:
[0024] Wetting the steel slag with water;
[0025] Mix the moistened steel slag with rubber powder.
[0026] As an improvement of the above technical solution, in the step of spraying a second high-viscosity modified emulsified asphalt on the surface of the second intermediate layer to obtain the surface layer, the second high-viscosity modified emulsified asphalt includes 8 to 12 wt% of an anti-icing and snow-melting agent;
[0027] The anti-icing and snow-melting agent is selected from one or more of urea, sodium acetate, magnesium acetate and calcium acetate.
[0028] As an improvement of the above technical solution, the anti-icing and snow-melting agent is a mixture of urea, sodium acetate and calcium acetate, and the weight ratio of urea, sodium acetate and calcium acetate is 4:2:1 to 6:4:3.
[0029] As an improvement of the above technical solution, the thickness of the road SGF ultra-thin anti-skid layer is ≤6mm, its structural depth is ≥0.6mm, and the swing value is ≥55BPN or the SFC value is ≥55.
[0030] Correspondingly, the present invention also discloses an SGF ultra-thin anti-skid layer for roads, which is prepared by the above-mentioned preparation method.
[0031] The implementation of the present invention has the following beneficial effects:
[0032] 1. In the preparation method of the road SGF ultra-thin anti-skid layer of the present invention, the first high-viscosity modified emulsified asphalt is first sprayed on the road surface, and then the steel slag rubber powder mixture and glass fiber are spread. After the first high-viscosity modified emulsified asphalt is demulsified, it is compacted, and finally a layer of the second high-viscosity modified emulsified asphalt is sprayed. After standing to form strength, the road SGF ultra-thin anti-skid layer can be obtained. Among them, the steel slag rubber powder mixture is obtained by mixing single-stage steel slag and rubber powder. Based on the above-mentioned preparation method of the present invention, on the one hand, the high-viscosity modified emulsified asphalt is separated from the steel slag rubber powder mixture, and the steel slag rubber powder mixture can be directly spread by a spreading process, without the need to mix steel slag, rubber powder, and high-viscosity modified emulsified asphalt first, and there is no need to consider the demulsification time and demulsification temperature of the mixture, which greatly reduces the stringent requirements for construction conditions. Second, using single-stage steel slag as the main aggregate lays a good foundation for uniform paving and subsequent high-pressure compaction, and improves the various properties of the ultra-thin anti-skid layer. Thirdly, by introducing rubber powder and glass fiber, the weather resistance and self-healing properties of the SGF ultra-thin anti-skid layer are improved. At the same time, the bonding performance between steel slag and high-viscosity modified emulsified asphalt is also improved, effectively preventing delamination and cracking. The thickness of the SGF ultra-thin anti-skid layer is reduced. Specifically, the thickness of the SGF ultra-thin anti-skid layer of the present invention can be reduced to less than 6 mm.
[0033] 2. In the SGF ultra-thin anti-skid layer of the road of the present invention, an anti-icing and snow-melting agent is introduced into the high-viscosity modified emulsified asphalt of the surface layer. The anti-icing and snow-melting agent has excellent compatibility with the high-viscosity modified emulsified asphalt, improves the overall adhesion and effectively lowers the freezing point (≤-4°C). At the same time, the non-traditional salt snow-melting component reduces road corrosion and water stability diseases.
[0034] 3. The SGF ultra-thin anti-skid layer of the road of the present invention can be made of steel slag, recycled rubber powder from waste tires, and recycled glass fiber from waste glass. The raw materials are easy to obtain, low in cost, and realize the resource utilization of solid waste. In addition, the construction of the present invention is carried out at room temperature, has no irritating odor, and is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a flow chart of the method for preparing the SGF ultra-thin anti-skid layer of the road in the present invention. DETAILED DESCRIPTION
[0036] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0037] refer to Figure 1 The present invention provides a method for preparing an SGF ultra-thin anti-skid layer of a road, which comprises the following steps:
[0038] S1: spraying the first high-viscosity modified emulsified asphalt on the road surface to form a high-viscosity modified emulsified asphalt layer;
[0039] S2: before the first high-viscosity modified emulsified asphalt is demulsified, the steel slag rubber powder mixture and the glass fiber are spread on the high-viscosity modified emulsified asphalt layer to obtain a first intermediate layer;
[0040] S3: After the first high-viscosity modified emulsified asphalt is demulsified, a rubber-wheeled roller is used to roll and knead the first intermediate layer and the high-viscosity modified emulsified asphalt layer so that the first intermediate layer and the high-viscosity modified emulsified asphalt layer penetrate and bond with each other to obtain a second intermediate layer;
[0041] S4: spraying the second high-viscosity modified emulsified asphalt on the surface of the second intermediate layer to obtain a surface layer;
[0042] S5: After the second highest viscosity modified emulsified asphalt is completely demulsified, it is allowed to stand for 1 to 2 hours to develop strength, and the road SGF ultra-thin anti-skid layer is obtained.
[0043] Based on the above-mentioned preparation method, one is to spray the first high-viscosity modified emulsified asphalt, spread the steel slag rubber powder mixture, glass fiber, and spray the second high-viscosity modified emulsified asphalt. The process of applying the high-viscosity modified emulsified asphalt and the main aggregate (steel slag) is separated, which greatly simplifies the construction process and reduces the performance requirements for various materials. Specifically, in conventional mixed asphalt materials (asphalt + aggregate + mineral powder, etc.), the demulsification time is generally required to be ≤120s, while the present invention has no special requirements for the demulsification time of the high-viscosity modified emulsified asphalt. Second, using single-stage steel slag as the main aggregate lays a good foundation for uniform paving and subsequent high-pressure compaction, and improves the various properties of the ultra-thin cover. Third, by introducing rubber powder and glass fiber, the weather resistance and self-healing properties of the SGF ultra-thin anti-skid layer are improved. At the same time, the bonding performance between steel slag and high-viscosity modified emulsified asphalt is also improved, which effectively prevents delamination and cracking, and reduces the thickness of the SGF ultra-thin anti-skid layer.
[0044] The present invention has relatively low requirements for high-viscosity modified emulsified asphalt, so a high-viscosity modified emulsified asphalt with a demulsification rate of fast, medium or slow can be selected. Preferably, in one embodiment, a high-viscosity modified emulsified asphalt with a demulsification rate of medium is selected to provide a reasonable time for the rolling and kneading process in step S3, thereby improving the various properties of the SGF ultra-thin anti-skid layer.
[0045] Specifically, the high-viscosity modified emulsified asphalt in the present invention has high viscosity, that is, the dynamic viscosity of the emulsified asphalt raw material before dilution at 60° C. is ≥200,000 Pa·s.
[0046] Specifically, in order to meet the requirements of spraying the first high-viscosity modified emulsified asphalt at room temperature, the demulsification speed is medium cracking, and the first high-viscosity modified emulsified asphalt has a high bonding strength to steel slag and glass fiber, the first high-viscosity modified emulsified asphalt is controlled to have an Engla viscosity of 1 to 10s at 25°C, a needle penetration of 40 to 120 (0.1mm), a softening point of ≥50°C, and an elongation of ≥20cm at 5°C. The solid content is controlled to be ≥65wt%.
[0047] Accordingly, in order to meet the requirements of spraying the second high viscosity modified emulsified asphalt at room temperature and having a high bonding strength to steel slag and glass fiber, in the present invention, the viscosity of the second high viscosity modified emulsified asphalt at 25°C is controlled to be 1-10s, the needle penetration is 40-120 (0.1mm), the softening point is ≥50°C, and the elongation at 5°C is ≥20cm. The solid content is controlled to be 40wt%-50wt%.
[0048] Specifically, the first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt in the present invention can be SBS high-viscosity modified emulsified asphalt, SBR high-viscosity modified emulsified asphalt or SBS, SBR composite high-viscosity modified emulsified asphalt. The above-mentioned high-viscosity modified emulsified asphalt has high bonding strength and can effectively avoid interlayer cracking. Preferably, in one embodiment of the present invention, the high-viscosity modified emulsified asphalt is SBS, SBR composite high-viscosity modified emulsified asphalt, and the weight ratio of SBS to SBR is (3-7): (2-4). Exemplary are 3.3:2.5, 3.7:2.7, 4.6:2.9, 5.7:3.3, 6.4:3.5 or 6.9:3.7, but not limited to this.
[0049] Among them, the steel slag rubber powder mixture is a mixture of single-stage steel slag and rubber powder. Single-stage steel slag refers to steel slag with a particle size within a single range. For example, the single-stage steel slag can be a single-stage steel slag with a particle size of 3 to 6 mm, or a single-stage steel slag with a particle size of 4 to 7 mm, but it is not limited thereto. Single-stage steel slag is convenient for spreading by a spreading process in the later stage, and is also convenient for compacting by a rubber-wheel roller with a larger pressure in the later stage, thereby improving the various properties of the road SGF ultra-thin anti-skid layer. In addition, steel slag itself has the advantages of low cost, high strength, good wear resistance and durability, and because it is a porous material, it has stronger adhesion to the first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt. In addition, steel slag also has the characteristics of greater structural depth and better anti-skid performance relative to ordinary crushed stone. Preferably, in one embodiment, the particle size of the single-stage steel slag is 4 to 7 mm, and the anti-skid performance of the road SGF ultra-thin anti-skid layer prepared therefrom is better.
[0050] Specifically, since steel slag is a porous structure, by mixing rubber powder and steel slag in advance, the rubber powder can form a uniform adhesion layer on the surface of the steel slag, which is convenient for bridging with the high-viscosity modified emulsified asphalt layer in the later stage to form a higher bonding strength and prevent stratification. It can also effectively resist the influence of extreme climate and weather under heavy load and heavy traffic conditions in high humidity and high heat areas. Specifically, the rubber powder can be waste rubber powder obtained by crushing waste tires, but is not limited to this. In order to form a uniform adhesion layer, the maximum particle size of the rubber powder is controlled to be ≤80 mesh sieve aperture, that is, the rubber powder can all pass through the 80 mesh sieve without sieve residue. Preferably, the maximum particle size of the rubber powder is controlled to be ≤100 mesh sieve aperture. When the particle size is smaller, the pore permeability to the steel slag surface is stronger and the bonding effect is stronger.
[0051] Specifically, the weight ratio of steel slag to rubber powder in the steel slag rubber powder mixture is 100: (1-3). When the amount of rubber powder is too much, part of the rubber powder is difficult to fully adhere to the surface of the steel slag, and it will be deposited at the bottom of the steel slag rubber powder mixture, which is easily blown away when spreading, and some will form agglomerates, making it difficult to effectively improve the adhesion effect. When the amount of rubber powder is small, the bonding effect between the steel slag and the tempered asphalt layer at the bottom is poor. Exemplary are 100: 1.5, 100: 2, 100: 2.5 or 100: 2.8, but not limited thereto. Preferably, the weight ratio of steel slag to rubber powder in the steel slag rubber powder mixture is 100: (1.5-2.5), and more preferably 100: 2.
[0052] Specifically, in order to achieve a good mixing of steel slag and rubber powder, in one embodiment of the present invention, the steel slag is first moistened with water, and then the moistened steel slag is mixed with the rubber powder. Herein, moistening refers to adding a small amount of water to form a water film on the surface of the steel slag. Specifically, the amount of water used for moistening is 0.5 to 3 wt% of the weight of the steel slag. When too much water is used for moistening, it is easy to penetrate and dilute the first high-viscosity modified emulsified asphalt at the bottom, weakening the bonding effect between the two. When less water is used for moistening, the mixing uniformity of the steel slag and the rubber powder is poor.
[0053] Among them, glass fiber is a common short-cut fiber in the field, which can improve the weather resistance and adhesion of the extremely thin anti-skid layer of the road SGF, and can also give it self-healing properties, effectively resisting the influence of extreme climate under heavy load and heavy traffic conditions in high humidity and high heat areas. Specifically, the length of the glass fiber is 5 to 50 mm, and exemplary ones are 5 mm, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm or 45 mm, but not limited thereto. Preferably, in one embodiment, the length of the glass fiber is 10 to 20 mm.
[0054] Specifically, the weight ratio of the steel slag mixture to the glass fiber is 100:0.2 to 100:1. When the amount of glass fiber is too large, it is difficult to achieve uniform mixing and bonding of the materials by rolling and kneading with a rubber-wheeled roller, and the various properties of the road SGF ultra-thin anti-skid layer are weak. When the amount of glass fiber is too small, the self-healing performance of the road SGF ultra-thin anti-skid layer is poor and the service life is short. Exemplarily, the weight ratio of the steel slag mixture to the glass fiber is 100:0.35, 100:0.4, 100:0.5, 100:0.6, 100:0.7 or 100:0.8, but is not limited thereto.
[0055] Specifically, in step S1, the spraying amount of the first high-viscosity modified emulsified asphalt is 1 to 1.2 L / m 2 When the spraying amount is too small, the bonding effect on the steel slag rubber powder mixture is poor. When the spraying amount is too large, the high-viscosity modified emulsified asphalt introduces more water, the water content in the first intermediate layer is large, the demulsification time is correspondingly longer, and the construction efficiency is reduced. For example, the spraying amount of the first high-viscosity modified emulsified asphalt is 1.0L / m 2 , 1.02L / m 2 , 1.06L / m 2 , 1.1L / m 2 , 1.14L / m 2 or 1.18 L / m 2 , but not limited to this. Preferably it is 1 to 1.12 L / m 2 .
[0056] Specifically, in step S1, the first high-viscosity modified emulsified asphalt can be sprayed by a commonly used spreading vehicle in the art, or by a synchronous crushed stone sealing vehicle. When the synchronous crushed stone sealing vehicle is used for spraying, the first high-viscosity modified emulsified asphalt is sprayed and the steel slag rubber powder mixture and the glass fiber are spread simultaneously, that is, the first high-viscosity modified emulsified asphalt is first sprayed by a nozzle arranged at the front end, and then the steel slag rubber powder mixture and the glass fiber are spread respectively by two discharging devices arranged at the rear end, that is, an integrated spraying and spreading is completed.
[0057] Preferably, in one embodiment, before spraying the first high-viscosity modified emulsified asphalt, the road surface may be cleaned, milled, etc. according to specific road conditions, but not limited thereto.
[0058] Specifically, in step S2, the total spreading amount of the steel slag rubber powder mixture and the glass fiber is 10-12 kg / m 2When the spreading amount is too much, it is difficult to achieve sufficient mixing, penetration and bonding of the steel slag rubber powder mixture, glass fiber and the first high-viscosity modified emulsified asphalt by simple roller rolling and kneading. When the spreading amount is small, the overall performance of the road SGF ultra-thin anti-skid layer is weak and the service life is short. For example, the total spreading amount of the steel slag rubber powder mixture and glass fiber is 10.4kg / m 2 , 10.8kg / m 2 , 11.2kg / m 2 , 11.4kg / m 2 , 11.6kg / m 2 or 11.8kg / m 2 , but not limited to this.
[0059] Specifically, in step S2, a paving machine commonly used in the art can be used to spread the steel slag rubber powder mixture and the glass fiber respectively, or a synchronous crushed stone sealing vehicle can be used to simultaneously spray the first high-viscosity modified emulsified asphalt and spread the steel slag rubber powder mixture and the glass fiber, but it is not limited thereto. When the steel slag rubber powder mixture and the glass fiber are spread by synchronous crushed stone sealing vehicle, there is no order of spreading the steel slag rubber powder mixture and the glass fiber. Preferably, in one embodiment, the glass fiber is spread first, and then the steel slag rubber powder mixture is spread to prevent the glass fiber from being blown away.
[0060] Specifically, in step S3, a rubber-wheeled roller of more than 26 tons is used to roll and knead the first intermediate layer. In order to achieve sufficient penetration and bonding between the first intermediate layer and the high-viscosity modified emulsified asphalt layer, the rolling times should be controlled to be ≥2 times, preferably, 2 to 3 times. It should be noted that in general ultra-thin overlays, since most of the asphalt mixture is compacted, the rubber-wheeled roller is generally ≤18 tons. The road SGF ultra-thin anti-skid layer structure of the present invention can be rolled by a higher tonnage roller, which optimizes various performances.
[0061] Preferably, in one embodiment of the present invention, after the rubber-wheel roller is used for treatment, the unadhered steel slag on the working surface can be recovered by an aggregate recovery vehicle. In addition, if there is a leak, the material should be laid and the supplemented material should be compacted.
[0062] Specifically, in step S4, a spreading vehicle may be used to spray the second high-viscosity modified emulsified asphalt, but the present invention is not limited thereto. The spraying amount of the second high-viscosity modified emulsified asphalt is 0.3 to 0.5 L / m 2 ; Exemplary is 0.32L / m 2 、0.38L / m 2 , 0.42L / m 2 , 0.44L / m 2 , 0.46L / m 2or 0.48 L / m 2 , but not limited to this.
[0063] Preferably, in one embodiment of the present invention, in step S5, the second high-viscosity modified emulsified asphalt also includes 8 to 12 wt% of an anti-icing and snow-melting agent, which can be selected from one or more of urea, sodium acetate, magnesium acetate, and calcium acetate. The above-mentioned anti-icing and snow-melting agent has good compatibility with the second high-viscosity modified emulsified asphalt, can improve the overall adhesion of the road SGF ultra-thin anti-skid layer, and can also effectively lower the freezing point and reduce road icing; in addition, the above-mentioned anti-icing and snow-melting agent of the present invention. Preferably, in one embodiment, the anti-icing and snow-melting agent is a mixture of urea, sodium acetate, and calcium acetate, and the weight ratio of urea, sodium acetate, and calcium acetate is 4:2:1 to 6:4:3. Based on this anti-icing and snow-melting agent, the freezing point can be lowered to -8°C.
[0064] Based on the above preparation method and selection of various components, the thickness of the road SGF ultra-thin anti-skid layer of the present invention is ≤6mm, its structural depth is ≥0.6mm, and its swing value is ≥55BPN or SFC value is ≥55.
[0065] The present invention will be further described below with specific embodiments:
[0066] Example 1
[0067] This embodiment provides an SGF ultra-thin anti-skid layer for roads, and the specific preparation method thereof is as follows:
[0068] 1. Wet the single-stage steel slag with a particle size of 4-7 mm with 0.3wt% of its weight of water, and then mix it evenly with the rubber powder (passed through a 100-mesh sieve) obtained by crushing waste tires, so that the rubber powder is evenly coated on the surface of the steel slag to obtain a steel slag rubber powder mixture. The amount of rubber powder used is 2wt% of the weight of the steel slag.
[0069] 2. Use synchronous crushed stone to seal the car. The first SBS high-viscosity modified emulsified asphalt (solid content 70wt%, SBS content 6wt%, 25℃ Engla viscosity 4s, needle penetration 65 (0.1mm), softening point 60℃, elongation 22cm at 5℃) is heated to 1.05L / m 2 The spraying amount is sprayed on the road surface, and the steel slag rubber powder mixture and glass fiber are spread at the same time. The total spreading amount of the two is 12kg / m 2 The weight ratio of steel slag to rubber powder in the steel slag-rubber powder mixture is 100:2, and the weight ratio of the steel slag-rubber powder mixture to glass fiber is 100:1.
[0070] 3. Use a rubber-wheeled roller of more than 26 tons to demulsify the first SBS high-viscosity modified emulsified asphalt, rub it repeatedly for 3 times, and then use the aggregate recovery vehicle to recover the steel slag rubber powder mixture and glass fiber that are not adhered to the working surface;
[0071] 4. Emulsified asphalt spreading vehicle at 0.4L / m 2 The second SBS high-viscosity modified emulsified asphalt (the first SBS high-viscosity modified emulsified asphalt is diluted to a solid content of 45wt%) is evenly spread on the entire working surface as a protective layer. After complete demulsification, it is allowed to stand for 1 to 2 hours to develop strength.
[0072] The road SGF ultra-thin anti-skid layer was just completed, and the subsequent phased tests were conducted after 1 month, 3 months, 6 months, and 12 months of normal traffic operation. The test results are as follows:
[0073] Example 1 0 1 month 3 months 6 months 12 months Construction depth TD(mm) 0.4 1.5 1.2 1.1 1.1 Lateral force coefficient SFC 22 63 65 73 76
[0074] Example 2
[0075] This embodiment provides an SGF ultra-thin anti-skid layer for roads, which differs from the embodiment 1 in that:
[0076] The steel slag is a single-stage steel slag with a particle size of 3 to 6 mm, and the rubber powder is a rubber powder that has passed through an 80-mesh sieve. The rest is the same as in Example 1.
[0077] The road SGF ultra-thin anti-skid layer was just completed, and the subsequent phased tests were conducted after 1 month, 3 months, 6 months, and 12 months of normal traffic operation. The test results are as follows:
[0078] Example 2 0 1 month 3 months 6 months 12 months Construction depth TD(mm) 0.4 1.1 0.9 0.8 0.8 Lateral force coefficient SFC 22 60 60 67 69
[0079] Example 3
[0080] This embodiment provides an SGF ultra-thin anti-skid layer for roads, which differs from the embodiment 1 in that the weight ratio of steel slag to rubber powder in the steel slag rubber powder mixture is 100:3. The rest is the same as the embodiment 1.
[0081] The road SGF ultra-thin anti-skid layer was just completed, and the subsequent phased tests were conducted after 1 month, 3 months, 6 months, and 12 months of normal traffic operation. The test results are as follows:
[0082] Example 3 0 1 month 3 months 6 months 12 months Construction depth TD(mm) 0.4 1.4 1.3 1.1 1.1 Lateral force coefficient SFC 22 64 67 71 75
[0083] Example 4
[0084] This embodiment provides an SGF ultra-thin anti-skid layer for roads, which differs from Embodiment 1 in that: in step 4, the second high-viscosity modified emulsified asphalt includes 10wt% anti-icing and snow-melting agent, which is a mixture of urea, sodium acetate and calcium acetate, and the weight ratio of urea, sodium acetate and calcium acetate is 5:3:2.
[0085] The road SGF ultra-thin anti-skid layer was just completed, and the subsequent phased tests were conducted after 1 month, 3 months, 6 months, and 12 months of normal traffic operation. The test results are as follows:
[0086] Example 1 0 1 month 3 months 6 months 12 months Construction depth TD(mm) 0.4 1.6 1.3 1.2 1.2 Lateral force coefficient SFC 22 65 68 77 79
[0087] Comparative Example 1
[0088] This comparative example provides an anti-slip cover surface, which differs from Example 1 in that the weight ratio of 3-6 mm steel slag and 4-7 mm steel slag is 40:60.
[0089] After using the above steel slag, 1.2L / m 2 Only by spraying a certain amount of high-viscosity modified emulsified asphalt can a road surface with good appearance be formed.
[0090] The test was conducted immediately after the veneer was completed, and after 1 month, 3 months, 6 months, and 12 months of normal traffic operation. The test results are as follows:
[0091] Comparative Example 1 0 1 month 3 months 6 months 12 months Construction depth TD(mm) 0.4 0.9 0.6 0.5 0.4 Lateral force coefficient SFC 22 42 38 35 29
[0092] Comparative Example 2.
[0093] This comparative example provides an anti-slip cover surface, which differs from Example 1 in that basalt is used instead of steel slag, and the rest is the same as Example 1.
[0094] The test was conducted immediately after the veneer was completed, and after 1 month, 3 months, 6 months, and 12 months of normal traffic operation. The test results are as follows:
[0095] Comparative Example 2 0 1 month 3 months 6 months 12 months Construction depth TD(mm) 0.4 0.9 0.8 0.8 0.6 Lateral force coefficient SFC 22 60 58 55 55
[0096] It can be seen from the above examples that the preparation method and material selection of the present invention can ensure that when an extremely thin SGF anti-skid layer (≤6mm) is used for roads with a very small thickness, its structural depth and anti-skid performance are better. Moreover, the preparation method of the present invention is simpler, more stable and more efficient. In addition, it can be seen from the comparison of the comparative examples and the embodiments that compared with conventional basalt, steel slag has better structural depth and anti-skid performance, and its wear resistance and durability under long-term service are significantly better than basalt.
[0097] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A method for preparing an ultra-thin SGF anti-skid layer for roads, characterized in that: include: Spray the first high-viscosity modified emulsified asphalt on the road surface to form a high-viscosity modified emulsified asphalt layer; wherein the spraying amount is 1 to 1.2 L / m 2 ; Before the first high-viscosity modified emulsified asphalt is demulsified, the steel slag rubber powder mixture and glass fiber are spread on the high-viscosity modified emulsified asphalt layer to obtain a first intermediate layer; wherein the steel slag rubber powder mixture is a mixture of single-stage steel slag and rubber powder; the total spreading amount of the steel slag rubber powder mixture and glass fiber is 10-12 kg / m 2 The weight ratio of steel slag to rubber powder in the steel slag-rubber powder mixture is 100:1 to 100:3, and the weight ratio of the steel slag-rubber powder mixture to glass fiber is 100:0.2 to 100:1; After the first high-viscosity modified emulsified asphalt is demulsified, a rubber-wheeled roller is used to roll and knead the first intermediate layer and the high-viscosity modified emulsified asphalt layer so that the first intermediate layer and the high-viscosity modified emulsified asphalt layer penetrate and bond with each other to obtain a second intermediate layer; The second high-viscosity modified emulsified asphalt is sprayed on the surface of the second intermediate layer to obtain a surface layer; wherein the spraying amount is 0.3-0.5 L / m 2 ; After the second high-viscosity modified emulsified asphalt is completely demulsified, it is left to stand for 1 to 2 hours to form strength, and the SGF ultra-thin anti-skid layer of the road is obtained. Wherein, the solid content of the first high-viscosity modified emulsified asphalt is greater than the solid content of the second high-viscosity modified emulsified asphalt.
2. The method for preparing the road SGF ultra-thin anti-skid layer as claimed in claim 1, characterized in that: The steel slag is selected from single-stage steel slag with a particle size of 3 to 6 mm or single-stage steel slag with a particle size of 4 to 7 mm; and / or The rubber powder is obtained by crushing waste tires, and its maximum particle size is ≤ the aperture of the 80-mesh sieve; and / or The length of the glass fiber is 5 to 50 mm.
3. The method for preparing the SGF ultra-thin anti-skid layer of a road as claimed in claim 1, characterized in that: The first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt have an Engla viscosity of 1 to 10 seconds at 25°C, a needle penetration of 40 to 120 (0.1 mm), a softening point of ≥50°C, and an elongation of ≥20 cm at 5°C; The solid content of the first high-viscosity modified emulsified asphalt is ≥65wt%, and the solid content of the second high-viscosity modified emulsified asphalt is 40-50wt%.
4. The method for preparing the SGF ultra-thin anti-skid layer of a road as claimed in claim 1, characterized in that: The first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt are selected from SBS high-viscosity modified emulsified asphalt, SBR high-viscosity modified emulsified asphalt or SBS, SBR composite high-viscosity modified emulsified asphalt.
5. The method for preparing the SGF ultra-thin anti-skid layer of a road as claimed in any one of claims 1 to 4, characterized in that: The steel slag is selected from single-stage steel slag with a diameter of 4 to 7 mm; and / or The rubber powder is obtained by crushing waste tires, and its maximum particle size is ≤ the aperture of a 100-mesh sieve; and / or The length of the glass fiber is 10 to 20 mm; and / or The first high-viscosity modified emulsified asphalt and the second high-viscosity modified emulsified asphalt are SBS and SBR composite high-viscosity modified emulsified asphalt, and the weight ratio of SBS to SBR is 3:2 to 7:
4.
6. The method for preparing the SGF ultra-thin anti-skid layer of a road as claimed in claim 1, characterized in that: The preparation method of the steel slag rubber powder mixture is: Wetting the steel slag with water; Mix the moistened steel slag with rubber powder.
7. The method for preparing the SGF ultra-thin anti-skid layer for roads as claimed in any one of claims 1 to 4 and 6, characterized in that: In the step of spraying a second high-viscosity modified emulsified asphalt on the surface of the second intermediate layer to obtain a surface layer, the second high-viscosity modified emulsified asphalt includes 8 to 12 wt% of an anti-icing and snow-melting agent; The anti-icing and snow-melting agent is selected from one or more of urea, sodium acetate, magnesium acetate and calcium acetate.
8. The method for preparing the SGF ultra-thin anti-skid layer of a road as claimed in claim 7, characterized in that: The anti-icing and snow-melting agent is a mixture of urea, sodium acetate and calcium acetate, and the weight ratio of urea, sodium acetate and calcium acetate is 4:2:1 to 6:4:
3.
9. The method for preparing the SGF ultra-thin anti-skid layer of a road as claimed in claim 1, characterized in that: The thickness of the road SGF ultra-thin anti-skid layer is ≤6mm, its structural depth is ≥0.6mm, and its swing value is ≥55BPN or SFC value is ≥55.
10. A road SGF ultra-thin anti-skid layer, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preventive maintenance material for asphalt pavement
CN102153315A
Surface treatment method for achieving low noise and skid resistance of road
CN106012746A
Composite road maintenance overlay construction process
CN111155402A
Ultra-thin wearing layer paving method based on high-viscosity emulsified asphalt
CN115057657A