Construction method of rubber improved soil shock insulation layer for frame structure
By using rubber to improve the soil isolation layer in house construction, combined with the inverted conical pit structure, the problem of insufficient compressive strength of the existing mixture of rubber particles and silty clay under earthquake action is solved, and the isolation effect and Seismic performance.
Patent Information
- Application Number
- CN202410730524.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-11
AI Technical Summary
The existing mixture of rubber particles and silty clay has poor compressive strength under earthquake action, which can easily lead to static settlement and overall overturning, and the isolation effect is poor.
The construction method of rubber-improved soil isolation layer is adopted, by compounding materials such as foundation pit soil, rubber particles, fly ash, quicklime, ferrous sulfate, hydrogen peroxide, citric acid, sodium citrate, fulvic acid and water. A rubber-modified soil with high compressive strength is generated, and an inverted conical pit is set at the bottom of the foundation pit to break down the earthquake intensity.
It significantly improves the compressive strength and seismic isolation effect of the rubber-improved soil layer, weakens the transmission intensity of seismic waves, and enhances the seismic performance of the frame structure.
Smart Images

Figure CN118756758A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of earthquake isolation of housing buildings, and in particular to a construction method of a rubber-modified soil earthquake isolation layer for a frame structure. Background Art
[0002] The rubber-improved soil obtained by mixing the rubber particles obtained by recycling and crushing waste tires with loess has good physical and mechanical properties while solving environmental pollution problems.
[0003] Rubber materials have been widely used in civil engineering. One of the methods is to combine waste rubber tires with sand and soil to form an economical and high-performance rubber tire structural foundation for small buildings. It has the advantages of simple structure, excellent environmental protection, reliable bearing capacity and low cost, which can greatly improve the safety factor of rural building structures. Another method is to mechanically crush waste rubber tires into fragments or particles, and then combine them with sand and soil in a certain proportion to form a new rubber sand or rubber soil mixture for application in actual engineering.
[0004] The mixture of rubber sand and rubber soil has the characteristics of strong elastic deformation performance, strong elastic recovery ability, light weight, small shear modulus, large damping, etc. It can be seen that rubber material is a new type of material with good performance and environmental protection.
[0005] A Chinese invention patent with publication number CN108951715A discloses a foundation isolation layer for village and town housing buildings. The isolation layer mixture includes rubber particles, fly ash and silty clay, and the rubber particle content is 30%; fly ash and silty clay are mixed in a ratio of 2:5, that is, the fly ash content is 20% and the silty clay content is 50%.
[0006] However, simply mixing rubber particles with silty clay will result in poor compressive strength of the soil, as the strength and stiffness of the rubber particles are lower than those of silty clay. Under the action of an earthquake, it is easy to produce large deformations, which may cause excessive static settlement of the upper structure and overall overturning in an earthquake, resulting in poor seismic isolation effect. Summary of the invention
[0007] In order to enhance the seismic isolation effect, the present application provides a construction method of a rubber-modified soil seismic isolation layer for a frame structure.
[0008] The present application provides a construction method for a rubber-modified soil seismic isolation layer for a frame structure, which adopts the following technical solution: A construction method for a rubber-modified soil seismic isolation layer for a frame structure comprises the following steps: S1: Excavate the foundation pit according to the normal construction process, and the depth should not be less than that of the ordinary foundation pit; S2: Backfill the foundation pit soil at the bottom of the foundation pit, then lay and compact the rubber improved soil, cover and maintain for 2 to 4 days to obtain the rubber improved soil seismic isolation layer; S3: Then a raft foundation is set above the rubber improved soil isolation layer, and a frame structure is set on the raft foundation; The rubber improved soil comprises foundation pit soil, rubber particles, fly ash, quicklime, ferrous sulfate, hydrogen peroxide, citric acid, sodium citrate, fulvic acid and water.
[0009] Preferably, the method for preparing the rubber-improved soil comprises the following steps: 1) drying and crushing the foundation pit soil to obtain raw soil, and uniformly mixing the raw soil, fly ash and rubber particles to obtain mixed soil; 2) After the humic acid solution, the mixed solution A and the mixed solution B are mixed evenly with the mixed soil, quicklime is added and mixed evenly to obtain rubber-improved soil; The fulvic acid solution comprises fulvic acid and water; The mixed solution A comprises ferrous sulfate, citric acid and water; The mixed solution B includes hydrogen peroxide, citric acid-sodium citrate and water.
[0010] Preferably, the volume ratio of the raw materials soil, fly ash, quicklime and rubber particles is 6-10:1.5-3.5:0.1-0.2:2-7.
[0011] Preferably, the dosage of the fulvic acid solution is 15 to 25 L / m 3 The dosage of the mixed solution A is 20 to 30 L / m 3 The dosage of the mixed solution B is 80-100 L / m 3 , the pH values of the mixed solution A and the mixed solution B are 3-5.
[0012] Preferably, the mass concentration of the fulvic acid solution is 40-60 g / L, the molar concentration of ferrous sulfate in the mixed solution A is 0.05-0.1 mol / L, and the molar concentration of hydrogen peroxide in the mixed solution B is 0.5-0.7 mol / L.
[0013] By adopting the above technical solution, fly ash has good cement activity and gelling properties, can fill the gaps between raw soil and rubber particles, and increase the bonding force and shear strength of the soil. The further addition of quicklime can stimulate the fly ash to generate hydration products with gelling properties. This is mainly because the main component of fly ash is acidic oxides, and its activity is most easily stimulated in alkaline media. Quicklime can not only provide an alkaline environment for the activation of fly ash activity, but also provide OH to break the Si-O and Al-O bonds in the fly ash glass. -It also provides the Ca required to activate the fly ash and hydrate it to form a hydraulic cementitious product. 2+ , while promoting the transformation of hydration products into more stable and stronger hydration products.
[0014] After fulvic acid solution, mixed liquor A, mixed liquor B are gradually mixed, calcium oxide meets water and generates calcium hydroxide, and under the effect of hydrogen peroxide and ferrous ion, fulvic acid can be mineralized to generate carbon dioxide, water and other inorganic states. This is mainly due to the fact that in the technical solution, under the catalytic action of ferrous sulfate, hydrogen peroxide can produce more hydroxyl radicals, thereby initiating and propagating free radical chain reactions, accelerating the oxidation of fulvic acid. And hydroxyl radicals have very high electronegativity or electrophilicity, and their electron affinity has very strong addition reaction characteristics. In the reaction process, ferric ion is generated at the same time, ferric ion can react with hydrogen peroxide to generate ferrous ion, and the ferrous ion generated reacts with hydrogen peroxide to generate hydroxyl radicals, and the hydroxyl radicals generated can further react with fulvic acid to generate organic free radicals, and organic free radicals are further oxidized, so that carbon chain breaks occur in organic structures, and finally oxidized to carbon dioxide and water. A portion of carbon dioxide can react with water to form carbonate and bicarbonate, which can combine with calcium ions in the soil to form calcium carbonate precipitates. Calcium hydroxide has a good capture effect on carbon dioxide, further generating calcium carbonate precipitates, which further solidifies the soil, making the compressive strength of the rubber-improved soil layer higher, thereby enhancing the seismic isolation effect of the frame structure.
[0015] Preferably, the quicklime is modified quicklime, and the preparation method of the modified quicklime comprises the following steps: The biochar, sodium hydroxide and water are mixed evenly, allowed to stand and soak, quicklime is added and mixed evenly, the solid and liquid are separated, washed and dried, sintered at 500-600° C. for 2-4 hours, cooled and crushed to obtain modified quicklime.
[0016] Preferably, the mass ratio of the biochar to quicklime is 1:2-5.
[0017] By adopting the above technical solution, the capture efficiency of carbon dioxide can be enhanced by modifying quicklime, and its adsorption properties are mainly reflected in solid phase physical adsorption and liquid phase chemical absorption. The porous structure and large amount of negatively charged surface of biochar can adsorb and fix carbon dioxide, so that carbon dioxide is retained in the soil, which can further promote the formation of calcium carbonate precipitation, improve the soil solidification strength, and make the rubber-modified soil layer have a higher compressive strength, thereby enhancing the seismic isolation effect of the frame structure.
[0018] Preferably, in step 2), a curing agent is also added to the fulvic acid solution, and the preparation method of the curing agent comprises the following steps: After monomer A, monomer B, 1-butene, polymerization inhibitor and water are mixed evenly, initiator is added and mixed evenly, the mixture is heated to 60-80°C, reacted for 4-6 hours, solid-liquid separation is performed, and drying is performed to obtain a curing agent; The molar mass ratio of the monomer A, the monomer B, and 1-butene is 0.5 to 2.5:1:1; The monomer A is at least one of methacrylic acid and 2-ethylacrylic acid; The monomer B is at least one of sodium methyl propylene sulfonate and sodium allyl sulfonate.
[0019] Preferably, the mass concentration of the curing agent in the fulvic acid solution is 30 to 50 g / L.
[0020] Preferably, the polymerization inhibitor is p-hydroxyanisole.
[0021] Preferably, the initiator is at least one of sodium persulfate, potassium persulfate and ammonium persulfate.
[0022] By adopting the above technical solution, a curing agent with a small molecular weight is obtained, which has strong permeability, can quickly polymerize soil molecules, make the soil condense into a granular structure, and improve the strength and stability of the rubber-improved soil layer. In addition, fly ash contains a lot of silicon dioxide, and the oxygen in silicon dioxide always bonds with two different silicon atoms to form a long silicon-oxygen chain or a three-dimensional grid. The super water absorption of the curing agent causes the surface hydroxyl groups between different silicon-oxygen chains to condense and dehydrate, resulting in cross-linking, which further solidifies the soil.
[0023] Preferably, in step S2, after partially backfilling the foundation pit soil at the bottom of the foundation pit, a foundation pit soil layer is obtained, and inverted cone holes arranged in a matrix are excavated at intervals on the foundation pit soil layer, and the inverted cone holes are filled and compacted with foundation improved soil, and then the rubber improved soil is laid and compacted; The foundation improved soil comprises foundation pit soil, rubber particles, calcium chloride, water glass, polyacrylamide and water.
[0024] Preferably, the longitudinal depth of the inverted cone pit is about 6 to 10 cm, the upper diameter of the inverted cone pit is about 7 to 12 cm, and the longitudinal and transverse spacings between the centers of adjacent inverted cone pits are 20 to 30 cm.
[0025] Preferably, the method for preparing the basic improved soil comprises the following steps: The foundation pit soil is dried and crushed to obtain raw soil, the raw soil and rubber particles accounting for 40-60% of the total volume of the raw soil and rubber particles are mixed evenly, and then the mixed liquid is added and mixed evenly to obtain foundation improved soil; The mixed solution is a mixed solution of calcium chloride, water glass, polyacrylamide and water.
[0026] Preferably, the amount of the mixed solution is 50 to 75 L / m 3 ; Preferably, the mass fraction of polyacrylamide in the mixed solution is 0.5-1.5%; Preferably, the mass fraction of calcium chloride in the mixed solution is 5 to 10%; Preferably, the mass fraction of the water glass is 3-7%.
[0027] By adopting the above technical solution, the inclined surface of the inverted cone pit can decompose the earthquake intensity transmitted from all directions into two components, longitudinal and lateral, which can weaken the earthquake intensity transmitted to the rubber improved soil isolation layer, thereby enhancing the isolation effect. By adding a mixed liquid to the foundation improved soil filled in the inverted cone pit, silica gel and calcium silicate gel can be generated in the soil, so that the soil is consolidated, thereby improving the strength and bearing capacity of the soil. In addition, the rubber particles in the foundation improved soil account for a large proportion, which can absorb and weaken part of the kinetic energy through its elastic deformation, further weaken the intensity of the upward propagation of seismic waves, and further enhance the isolation effect of the frame structure.
[0028] Preferably, the rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps: The rubber particles are mixed evenly with the alkali solution, left to stand for 18 to 24 hours, separated from the solid and the liquid, washed, mixed evenly with the silane coupling agent, silicone resin and water, then added with water glass, mixed evenly, separated from the solid and the liquid, and dried to obtain modified rubber particles.
[0029] Preferably, the amount of the silicone resin used is 2-8% of the total mass of the rubber particles.
[0030] Preferably, the amount of water glass used is 3-5% of the total mass of the rubber particles.
[0031] Preferably, the volume ratio of the rubber particles to the alkali solution is 1:1.5-2.5.
[0032] By adopting the above technical solution, since the bonding force between rubber particles and soil particles is poor, the roughness of the rubber particle surface can be enhanced by soaking in alkaline solution, which can not only enhance the bonding force between rubber particles and soil particles, but also improve the unconfined compressive strength of soil particles stabilized by rubber particles. By introducing silane coupling agent, silicone resin and water glass, the formation of a strong chemical bond between rubber particles or silicone resin and water glass can be improved, and the interfacial bonding strength can be improved. Water glass reacts with water to generate silica gel, which can improve the bonding force between rubber particles and soil particles; the sodium silicate in water glass combines with calcium ions in the soil to generate calcium silicate precipitation around the rubber particles, filling the gaps in the soil, improving the solidification of the soil, and enhancing the seismic isolation effect. The addition of silicone resin can improve the corrosion resistance of rubber particles in the soil, thereby improving the seismic isolation effect of the frame structure.
[0033] Preferably, in step S2, after the rubber improved soil isolation layer is cured, the rubber improved soil isolation layer is sprayed with 10 to 20 L / m 2 After spraying the alkali solution, leave it for 1 to 3 days.
[0034] Preferably, the alkali solution is a mixture of sodium hydroxide solution and sodium carbonate solution; The mass fraction of the sodium hydroxide in the alkali solution is 6-8%, and the mass fraction of the sodium carbonate in the alkali solution is 4-6%.
[0035] By adopting the above technical solution, by spraying a small amount of alkali solution, on the one hand, it can promote the conversion of carbon dioxide in the soil into carbonate ions, so that the carbonate ions can combine with the calcium ions in the soil. On the other hand, the alkali solution contains a small amount of carbonate ions, which can also further combine with the calcium ions in the soil, further increasing the proportion of calcium carbonate in the soil, enhancing the soil solidification effect, and thus improving the seismic isolation effect of the frame structure.
[0036] In summary, the present application includes at least one of the following beneficial technical effects: 1. By using fulvic acid solution, mixed solution A, mixed solution B, calcium oxide, fly ash, rubber particles and foundation pit soil for compound improvement, calcium carbonate precipitation is generated between rubber particles and soil particles and between soil particles, thereby improving the solidification performance and compressive strength of the soil, thereby enhancing the seismic isolation effect of the frame structure.
[0037] 2. The capture efficiency of carbon dioxide can be enhanced by modifying quicklime, so that carbon dioxide can be retained in the soil, which can further promote the formation of calcium carbonate precipitation, improve the soil solidification strength, and make the compressive strength of the rubber-improved soil layer higher, thereby enhancing the seismic isolation effect of the frame structure.
[0038] 3. By setting an inverted cone-shaped pit filled with foundation improvement soil under the rubber improved soil isolation layer, the earthquake intensity transmitted upward to the rubber improved soil isolation layer can be weakened, further enhancing the isolation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 (a) to (c) are the acceleration time history curves and Fourier spectra of three different seismic waves; Figure 2 (a) to (d) are the observed column height-absolute displacement curves in the frame structures of Examples 1 to 3 and Comparative Examples 1 to 5 under the action of an artificial seismic wave with an acceleration peak of 0.1 g; Figure 3 (a) to (d) are observed column height-maximum shear stress curves in the frame structures of Examples 1 to 3 and Comparative Examples 1 to 5 under the action of artificial seismic waves with an acceleration peak of 0.1 g; Figure 4 The column height-absolute displacement curves observed in the frame structures of Examples 1 to 3 and Comparative Example 1 under the action of an artificial seismic wave with an acceleration peak of 0.2g; Figure 5 (a) to (c) are the Fourier spectra of the observation columns in the frame structures of Comparative Example 1 and Example 2 under the action of three different seismic waves with a peak acceleration of 0.2g. DETAILED DESCRIPTION
[0040] The present application is further described in detail below with reference to the accompanying drawings and embodiments.
[0041] In the embodiment: The rubber particles are granular particles obtained by mechanically crushing waste tires. The main particle size range is 4 to 6 mm, and the average particle size is 5 mm. The raw soil comes from foundation pit soil.
[0042] The frame structure is a two-story frame structure with a length of 9.6m, a width of 5.6m and a floor height of 3m. The concrete in the frame structure, raft foundation and strip foundation adopts S4R units, the steel bars adopt T3D2 units, and the rubber improved soil isolation layer and foundation soil adopt C3D8R units.
[0043] The main chemical components of fly ash are 25.32% Al2O3, 49.65% SiO2, 7.50% Fe2O3, 5.3% CaO and 0.65% MgO.
[0044] The main chemical component of quicklime powder is 85.61% calcium oxide.
[0045] The rubber improved soil and foundation improved soil are prepared and used immediately, and the humic acid solution, mixed solution A, mixed solution B and mixed solution involved are all prepared and used immediately.
[0046] Table 1 Material parameters Material <![CDATA[Density (kg / m 3 )]]> Elastic modulus (MPa) Poisson's ratio Damping ratio Concrete 2500 32500 0.2 0.05 Foundation pit soil 1960 109.87 0.26 0.05 Rubber Improved Soil 1460~1490 50 0.49 0.3 Rebar 7850 206000 0.3 0.04 Example 1 This embodiment provides a construction method of a rubber improved soil seismic isolation layer for a frame structure, which comprises the following steps by weight: S1: excavating a foundation pit according to a common construction process, wherein the foundation pit is about 14 m long, 10 m wide and 8 m deep; S2: After the bottom of the excavated foundation pit is leveled, the foundation pit soil is backfilled and compacted in layers and leveled until the depth from the ground is about 1.9m. Then, the rubber improved soil is laid and compacted in layers and leveled, and then covered with plastic film and cured for 2 days to obtain the rubber improved soil seismic isolation layer; S3: A raft foundation is set above the rubber improved soil isolation layer, and a two-layer frame structure is set on the raft foundation; The thickness of the rubber-improved soil isolation layer is about 0.4m.
[0047] The method for preparing the rubber-improved soil in this embodiment comprises the following steps: 1. After drying and crushing the foundation pit soil, pass it through a 2mm sieve to obtain the raw soil. Take 0.6m 3 Raw soil, 0.15m 3 Fly ash, 0.2m 3 The rubber particles are mechanically stirred and mixed evenly to obtain mixed soil; 2. Mix the humic acid solution, mixed solution A and mixed solution B with the mixed soil in order, and then add 0.01m 3 Quicklime powder is mixed evenly with mechanical stirring to obtain rubber-improved soil.
[0048] The fulvic acid solution includes fulvic acid and water. The mass concentration of fulvic acid in the fulvic acid solution is 40 g / L and the dosage is 15 L / m 3 ; The dosage of mixed liquid A is 20L / m 3 The dosage of mixed liquid B is 80L / m 3 ; The humic acid solution, mixed solution A and mixed solution B are all evenly mixed with the mixed soil by spraying in small amounts multiple times.
[0049] Mixed solution A includes citric acid, ferrous sulfate and water, the molar concentration of ferrous sulfate in the mixed solution A is 0.05 mol / L, and the pH value is 3; Mixed solution B includes citric acid, sodium citrate, hydrogen peroxide and water. The molar concentration of hydrogen peroxide in mixed solution B is 0.5 mol / L, and the pH value is 3.
[0050] Example 2 The difference between this embodiment and embodiment 1 is that in step S2, the foundation pit soil is backfilled and compacted in layers and leveled until the depth from the ground is about 2.1 m, and the thickness of the rubber improved soil isolation layer is about 0.6 m.
[0051] The rest is the same as in Example 1.
[0052] Example 3 The difference between this embodiment and embodiment 2 is that in step S2, the foundation pit soil is backfilled and compacted in layers and leveled until the depth from the ground is about 2.3m, and the thickness of the rubber improved soil isolation layer is about 0.8m.
[0053] The rest is the same as in Example 2.
[0054] Example 4 The difference between this embodiment and embodiment 2 is that the mass concentration of the fulvic acid solution is 60 g / L, the molar concentration of ferrous sulfate in the mixed solution A is 0.1 mol / L, the molar concentration of hydrogen peroxide in the mixed solution B is 0.7 mol / L, and the pH of the mixed solution A and the mixed solution B is 5.
[0055] The rest is the same as in Example 2.
[0056] Example 5 The difference between this embodiment and embodiment 4 is that the mass concentration of the fulvic acid solution is 50 g / L, the molar concentration of ferrous sulfate in the mixed solution A is 0.08 mol / L, and the molar concentration of hydrogen peroxide in the mixed solution B is 0.6 mol / L.
[0057] The dosage of fulvic acid solution is 25L / m 3 ; The dosage of mixed liquid A is 30L / m 3 The dosage of mixed liquid B is 100L / m 3 , the pH of mixed solution A and mixed solution B is 4.
[0058] The rest is the same as Example 4.
[0059] Example 6 The difference between this embodiment and embodiment 5 is that: In step 2), the dosage of fulvic acid solution is 20 L / m 3 ; The dosage of mixed liquid A is 25L / m 3 The dosage of mixed liquid B is 90L / m 3 .
[0060] The quicklime is modified quicklime, and the preparation method of the modified quicklime comprises the following steps: 5 kg of biochar was mixed with 300 L of 8% sodium hydroxide solution by mass, and then allowed to stand for 2 hours. Then, 25 kg of quicklime powder was added, and the mixture was mixed and placed in an ultrasonic device for 2 hours of ultrasonic oscillation. The frequency of the ultrasonic wave was 40 KHz. After washing with clean water and drying, the mixture was sintered at 500 ° C for 4 hours, cooled to room temperature, and ground to obtain modified quicklime. In step 2), the amount of quicklime is 0.15m 3 .
[0061] The rest is the same as Example 5.
[0062] Example 7 The difference between this embodiment and embodiment 6 is that in step 2), the quicklime is modified quicklime, and the preparation method of the modified quicklime comprises the following steps: 10 kg of biochar was mixed with 300 L of 8% sodium hydroxide solution by mass, and then allowed to stand for 2 hours. Then, 20 kg of quicklime powder was added, and the mixture was mixed and placed in an ultrasonic device for 2 hours of ultrasonic oscillation at a frequency of 40 KHz. After washing with clean water and drying, the mixture was sintered at 600 ° C for 2 hours, cooled to room temperature, and ground to obtain modified quicklime. The rest is the same as Example 6.
[0063] Example 8 The difference between this embodiment and embodiment 7 is that in step 2), a curing agent is also added to the fulvic acid solution, and the mass concentration of the curing agent in the fulvic acid solution is 30 g / L.
[0064] The preparation method of the curing agent comprises the following steps: 0.5 mol of methacrylic acid, 1 mol of sodium allyl sulfonate, 1 mol of 1-butene and 500 ml of distilled water are mixed evenly, and then 0.05% of p-hydroxyanisole accounting for the total mass of methacrylic acid and sodium allyl sulfonate is added, and the mixture is stirred and mixed evenly, and then 0.8% of sodium persulfate accounting for the total mass of methacrylic acid and sodium allyl sulfonate is added, and the mixture is further stirred and mixed evenly, and the mixture is heated to 60° C., reacted for 6 hours, and distilled to a viscous state, and then 25% ammonia water by mass is gradually added dropwise, and the pH value is adjusted to neutral to obtain a transparent viscous solution, and then the transparent viscous solution is added dropwise to acetone, and the volume ratio of acetone to the transparent viscous solution is 5:1, filtered, and vacuum dried at 40° C. to obtain a curing agent.
[0065] The rest is the same as Example 7.
[0066] Example 9 The difference between this embodiment and embodiment 8 is that in step 2), the mass concentration of the curing agent in the fulvic acid solution is 50 g / L.
[0067] The preparation method of the curing agent comprises the following steps: 2.5 mol of 2-ethylacrylic acid, 1 mol of sodium methacrylic acid sulfonate, 1 mol of 1-butene and 1000 ml of distilled water are mixed evenly, and then 0.05% of p-hydroxyanisole accounting for the total mass of 2-ethylacrylic acid and sodium methacrylic acid sulfonate is added, and the mixture is stirred and mixed evenly. Then, 0.8% of potassium persulfate accounting for the total mass of 2-ethylacrylic acid and sodium methacrylic acid sulfonate is added, and the mixture is further stirred and mixed evenly. The mixture is heated to 80° C., reacted for 4 hours, and distilled to a viscous state. Then, 25% ammonia water by mass is gradually added dropwise, and the pH value is adjusted to neutral to obtain a transparent viscous solution. Then, the transparent viscous solution is added dropwise to acetone, and the volume ratio of acetone to the transparent viscous solution is 5:1. The mixture is filtered, and vacuum dried at 40° C. to obtain a curing agent.
[0068] The rest is the same as Example 8.
[0069] Example 10 The difference between this embodiment and embodiment 9 is that: In step S2, after the bottom of the excavated foundation pit is leveled, the foundation pit soil is backfilled and compacted in layers, and leveled until the depth from the ground is about 2.1m, to obtain a foundation pit soil layer, and inverted cone pits arranged in a matrix are excavated at intervals on the foundation pit soil layer, the longitudinal depth of the inverted cone pit is about 6cm, the upper diameter of the inverted cone pit is about 7cm, and the longitudinal and transverse spacings between the centers of adjacent inverted cone pits are 20cm. In the inverted cone pits, the foundation improved soil is filled and compacted, and then the rubber improved soil is laid and compacted in layers and leveled, and then covered with plastic film and cured for 4 days to obtain a rubber improved soil seismic isolation layer; The method for preparing foundation improved soil comprises the following steps: The foundation pit soil was dried and crushed, and then passed through a 2 mm sieve to obtain the raw soil. 3 Raw soil and 0.13m 3 The rubber particles are mechanically stirred and mixed evenly, and then added into the mixed liquid and mixed evenly to obtain the base improved soil; The dosage of the mixed liquid is 50L / m 3 ; The mass fraction of polyacrylamide in the mixed solution is 0.5%; The mass fraction of calcium chloride in the mixed solution is 5%; The mass fraction of water glass is 3%.
[0070] In step 2), the mass concentration of the curing agent in the fulvic acid solution is 40 g / L.
[0071] The preparation method of the curing agent comprises the following steps: 1.5 mol of methacrylic acid, 1 mol of sodium methacrylic acid sulfonate, 1 mol of 1-butene and 700 ml of distilled water are mixed evenly, and then 0.05% of p-hydroxyanisole accounting for the total mass of methacrylic acid and sodium methacrylic acid sulfonate is added, and the mixture is stirred and mixed evenly, and then 0.8% of ammonium persulfate accounting for the total mass of methacrylic acid and sodium methacrylic acid sulfonate is added, and the mixture is further stirred and mixed evenly, and the mixture is heated to 80° C., reacted for 4 hours, and distilled to a viscous state, and then 25% ammonia water by mass is gradually added dropwise, and the pH value is adjusted to neutral to obtain a transparent viscous solution, and then the transparent viscous solution is added dropwise to acetone, and the volume ratio of acetone to the transparent viscous solution is 5:1, filtered, and vacuum dried at 40° C. to obtain a curing agent.
[0072] The rest is the same as Example 9.
[0073] Embodiment 11 The difference between this embodiment and embodiment 10 is that: In step S2, the longitudinal depth of the inverted cone pit is about 10 cm, the upper diameter of the inverted cone pit is about 12 cm, and the longitudinal and transverse spacings between the centers of adjacent inverted cone pits are both 30 cm.
[0074] The method for preparing foundation improved soil comprises the following steps: The foundation pit soil was dried and crushed, and then passed through a 2 mm sieve to obtain the raw soil. 3 Raw soil and 0.3m 3 The rubber particles are mechanically stirred and mixed evenly, and then added into the mixed liquid and mixed evenly to obtain the base improved soil; The dosage of the mixed liquid is 75L / m 3 ; The mass fraction of polyacrylamide in the mixed solution is 1.5%; The mass fraction of calcium chloride in the mixed solution is 10%; The mass fraction of water glass is 7%.
[0075] In step 2), the mass concentration of the curing agent in the fulvic acid solution is 40 g / L.
[0076] The rest is the same as Example 10.
[0077] Example 12 The difference between this embodiment and embodiment 11 is that: In step S2: The method for preparing foundation improved soil comprises the following steps: The foundation pit soil was dried and crushed, and then passed through a 2 mm sieve to obtain the raw soil. 3 Raw soil and 0.2m 3The rubber particles are mechanically stirred and mixed evenly, and then added into the mixed liquid and mixed evenly to obtain the base improved soil; The dosage of the mixed liquid is 60L / m 3 ; The mass fraction of polyacrylamide in the mixed solution is 1%; The mass fraction of calcium chloride in the mixed solution is 8%; The mass fraction of water glass is 6%.
[0078] The rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps: 0.2m 3 The rubber particles were mixed evenly with 300 L of alkali solution, allowed to stand and soak for 24 h, filtered, washed with clean water until neutral, and then 500 L of KH-570 with a mass concentration of 1% was added. Then, 2% of methyl silicone resin and 3% of water glass based on the total mass of the rubber particles were added. The mixture was stirred for 30 min at a stirring speed of 800 r / min, filtered, placed in a drying oven, and dried at 50 ° C for 2 h to obtain modified rubber particles.
[0079] The mass fraction of sodium hydroxide in the alkali solution is 6%, and the mass fraction of sodium carbonate in the alkali solution is 4%.
[0080] The rest is the same as Example 11.
[0081] Embodiment 13 The difference between this embodiment and embodiment 12 is that: The rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps: 0.2m 3 The rubber particles were mixed evenly with 500 L of alkali solution, allowed to stand and soak for 18 h, filtered, washed with clean water until neutral, and then 500 L of KH-570 with a mass concentration of 1% was added. Then, 8% of the total mass of the rubber particles was added with methyl silicone resin and 5% of water glass was added to the total mass of the rubber particles. The mixture was stirred for 30 min at a stirring speed of 800 r / min, filtered, placed in a drying oven, and dried at 50°C for 2 h to obtain modified rubber particles.
[0082] The mass fraction of sodium hydroxide in the alkali solution is 8%, and the mass fraction of sodium carbonate in the alkali solution is 6%.
[0083] The rest is the same as Example 12.
[0084] Embodiment 14 The difference between this embodiment and embodiment 13 is that: The rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps: 0.2m3 The rubber particles were mixed evenly with 500 L of alkali solution, allowed to stand and soak for 20 h, filtered, washed with clean water until neutral, and then 500 L of KH-570 with a mass concentration of 1% was added. Then, 6% of methyl silicone resin and 5% of water glass based on the total mass of the rubber particles were added. The mixture was stirred for 30 min at a stirring speed of 800 r / min, filtered, placed in a drying oven, and dried at 50°C for 2 h to obtain modified rubber particles.
[0085] The mass fraction of sodium hydroxide in the alkali solution is 7%, and the mass fraction of sodium carbonate in the alkali solution is 5%.
[0086] In step S2, after the rubber improved soil isolation layer is cured, the rubber improved soil isolation layer is sprayed with 10L / m 2 After spraying the lye solution, cover with plastic film and leave it for 1 day.
[0087] The rest is the same as Example 13.
[0088] Embodiment 15 The difference between this embodiment and embodiment 14 is that: In step S2, after the rubber improved soil isolation layer is cured, the rubber improved soil isolation layer is heated at 20L / m 2 After spraying the lye solution, cover with plastic film and leave it for 3 days.
[0089] The rest is the same as Example 14.
[0090] Example 16 The difference between this embodiment and embodiment 15 is that: The method for preparing the rubber-improved soil in this embodiment comprises the following steps: 1. After drying and crushing the foundation pit soil, pass it through a 2mm sieve to obtain the raw soil. Take 0.8m 3 Raw soil, 0.35m 3 Fly ash, 0.5m 3 The rubber particles are mechanically stirred and mixed evenly to obtain mixed soil; 2. Mix the humic acid solution, mixed solution A and mixed solution B with the mixed soil in order, and then add 0.02m 3 Quicklime powder is mixed evenly with mechanical stirring to obtain rubber-improved soil.
[0091] The rest is the same as Example 15.
[0092] Embodiment 17 The difference between this embodiment and embodiment 16 is that: The method for preparing the rubber-improved soil in this embodiment comprises the following steps: 1. After drying and crushing the foundation pit soil, pass it through a 2mm sieve to obtain the raw soil. Take 1m 3 Raw soil, 0.25m 3 Fly ash, 0.7m 3 The rubber particles are mechanically stirred and mixed evenly to obtain mixed soil; 2. Mix the humic acid solution, mixed solution A and mixed solution B with the mixed soil in order, and then add 0.02m 3 Quicklime powder is mixed evenly with mechanical stirring to obtain rubber-improved soil.
[0093] The rest is the same as Example 16.
[0094] Embodiment 18 The difference between this embodiment and embodiment 17 is that: The method for preparing the rubber-improved soil in this embodiment comprises the following steps: 1. After drying and crushing the foundation pit soil, pass it through a 2mm sieve to obtain the raw soil. Take 1m 3 Raw soil, 0.25m 3 Fly ash, 0.8m 3 The rubber particles are mechanically stirred and mixed evenly to obtain mixed soil; 2. Mix the humic acid solution, mixed solution A and mixed solution B with the mixed soil in order, and then add 0.02m 3 Quicklime powder is mixed evenly with mechanical stirring to obtain rubber-improved soil.
[0095] The rest is the same as Example 17.
[0096] Comparative Example 1 This comparative example provides a construction method of a frame structure, which comprises the following steps by weight: S1: Excavate the foundation pit according to the normal construction process. The length of the foundation pit is about 14m, the width is about 10m, and the depth is about 8m; S2: After the bottom of the excavated foundation pit is leveled, the foundation pit soil is backfilled and compacted in layers and leveled until the depth from the ground is about 1.5m. The raft foundation is then set up, and a two-layer frame structure is set up on the raft foundation.
[0097] Comparative Example 2 The difference between this comparative example and comparative example 1 is that in step S2, after the bottom of the excavated foundation pit is leveled, the foundation pit soil is backfilled and compacted in layers and leveled until the depth from the ground is about 1.5m, and then a strip foundation is set up, and a two-layer frame structure is set on the strip foundation.
[0098] Other details are the same as those in Comparative Example 1.
[0099] Comparative Example 3 The difference between this comparative example and Example 1 is that in step S3, a strip foundation is arranged above the rubber improved soil isolation layer, and a two-layer frame structure is arranged on the strip foundation.
[0100] The rest is the same as in Example 1.
[0101] Comparative Example 4 The difference between this comparative example and Example 1 is that in step S2, the foundation pit soil is backfilled and compacted in layers and leveled until the depth from the ground is about 2.1 m, and the thickness of the rubber improved soil isolation layer is about 0.6 m.
[0102] The rest is the same as in Example 1.
[0103] Comparative Example 5 The difference between this comparative example and Example 1 is that in step S2, the foundation pit soil is backfilled and compacted in layers and leveled until the depth from the ground is about 2.3m, and the thickness of the rubber improved soil isolation layer is about 0.6m.
[0104] The rest is the same as in Example 1.
[0105] Performance Testing Finite element models are constructed for the buildings in Examples 1 to 18 and Comparative Examples 1 to 5, and the finite element models include a two-layer frame structure, a foundation (strip foundation or raft foundation), a rubber-improved soil isolation layer, foundation pit soil, and foundation improved soil. The rubber-improved soil is laid flat under the foundation, and the foundation improved soil is arranged under the rubber-improved soil layer. Using the finite element analysis software abaqus, the corresponding non-isolated and isolated structural analysis models are constructed based on this. The upper structure of this structural model is a two-layer frame structure with a length of 9.6m, a width of 5.6m, and a floor height of 3m. The soil body is 14m long, 10m wide, and 8m deep for equivalent linearization. The concrete in the frame structure and the foundation adopts S4R units, the steel bars adopt T3D2 units, and the rubber-improved soil and foundation soil adopt C3D8R units.
[0106] The constructed finite element model is used to simulate the seismic response of the two-story frame structure of Examples 1 to 18 and Comparative Examples 1 to 5. In order to facilitate the study of the influence of the rubber-modified soil isolation layer on the displacement of the frame structure, since the frame structure is a symmetrical structure, any column is taken as the observation column. In order to ensure the accuracy and reliability in the abaqus finite element simulation software, a viscoelastic artificial boundary is used for the soil boundary appearing in Examples 1 to 18 and Comparative Examples 1 to 5.
[0107] 1. Seismic wave selection When using the time history analysis method, the time history curves of actual strong earthquake records and artificially simulated acceleration should be selected according to the building site category and design earthquake grouping. Therefore, three earthquake waves suitable for Class II sites were selected for this analysis, two of which were actual strong earthquake records of The Friuli (Italy) earthquake of May 06, 1976 (hereinafter referred to as Friuli earthquake wave) and San Fernando, 2 / 9 / 1971, Santa Anita Dam (hereinafter referred to as San Fernando earthquake wave), and the other was an artificial wave synthesized according to the code response spectrum (hereinafter referred to as artificial earthquake wave). In order to study the peak acceleration of the original earthquake wave under the same peak acceleration earthquake wave, the peak acceleration of the original earthquake wave was adjusted to 0.2g and input into the building frame structure for calculation. The time history curve of the acceleration of the earthquake wave and the Fourier spectrum are shown in Figure 1 Because the viscoelastic artificial boundary is used in the finite element model in this paper, the input of the earthquake motion adopts the corresponding equivalent load input method. The seismic wave is in the form of a shear wave propagating vertically upward. The earthquake input method adopts the input method of equivalent node force. The velocity time history and displacement time history are obtained by integrating the acceleration time history and calculating the quadratic integral using the program.
[0108] Figure 1 Middle: (a) is the acceleration time history curve and Fourier spectrum of the Friuli earthquake wave; (b) is the acceleration time history curve and Fourier spectrum of the San Fernando earthquake wave; (c) is the acceleration time history curve and Fourier spectrum of the artificial seismic wave.
[0109] 2. Experimental testing 2.1 Effect of base contact area on seismic isolation effect The seismic response of the two-story frame structure in Examples 1 to 3 and Comparative Examples 1 to 5 was simulated and calculated. An artificial seismic wave with an acceleration peak of 0.1g was selected as the dynamic load. The artificial seismic wave was a shear wave propagating vertically upward, and was applied to the two-story frame structure in Examples 1 to 3 and Comparative Examples 1 to 5 by inputting an equivalent node force. The peak value of the vertex acceleration of the frame structure and the reduction amplitude (referred to as reduction amplitude) of the peak acceleration of the vertex under different foundation forms under the same thickness of the seismic isolation layer were obtained. The experimental test results are shown in Table 2.
[0110] Table 2 Peak acceleration and drop of the observation column in the frame structure in Examples 1 to 3 and Comparative Examples 1 to 5 <![CDATA[Peak acceleration (m / s 2 )]]> <![CDATA[Peak acceleration (m / s 2 )]]> Decrease (%) Comparative Example 2 3.26 Comparative Example 1 3.24 0.6 Comparative Example 3 2.87 Example 1 2.69 6.2 Comparative Example 4 2.54 Example 2 2.32 8.6 Comparative Example 5 2.26 Example 3 2.03 10.1 It can be seen from Table 2 that with the increase of the thickness of the rubber improved soil isolation layer, the reduction in the peak value of the vertex acceleration of the observation column in the structure using the raft foundation (Comparative Example 1 and Examples 1 to 3) compared with the strip foundation (Comparative Examples 2 to 5) gradually increases, that is, when the thickness of the rubber improved loess isolation layer is 0m, 0.4m, 0.6m and 0.8m, the reduction in the peak value of the vertex acceleration of the raft foundation form compared with the strip foundation form is 0.6%, 6.2%, 8.6% and 10.1%, respectively. Therefore, with the increase of the thickness of the rubber improved soil isolation layer, the isolation effect of the frame structure using the raft foundation is more significant.
[0111] In order to study the effect of the rubber-modified soil isolation layer on the displacement of the frame structure, an observation point is set every 1m for the observation column mentioned above, and the maximum displacement of each observation point is extracted to form a column height-absolute displacement curve. An artificial seismic wave with an acceleration peak of 0.1g is selected as the dynamic load. The artificial seismic wave is a shear wave that propagates vertically upward. The equivalent node force is applied to the two-story frame structure of Examples 1 to 3 and Comparative Examples 1 to 5 to obtain a column height-absolute displacement peak curve, as shown in FIG. Figure 2 As shown, the maximum displacement of the observation column in Examples 1 to 3 and Comparative Examples 1 to 5, as well as the maximum displacement difference under different foundation forms of the same thickness of the seismic isolation layer are recorded, and the results are shown in Table 3.
[0112] Depend on Figure 2 Qualitative analysis of (a) to (d) shows that: The column height-absolute displacement curves under the two foundation forms have the same trend of change, and the displacement increases with the increase of the height of the observation point. And the maximum displacement of the observation column under the two foundation forms decreases with the increase of the thickness of the rubber-improved soil isolation layer. This shows that increasing the thickness of the rubber-improved soil layer can effectively reduce the maximum displacement of the frame structure.
[0113] There is a gap between the column height-absolute displacement curves of the frame structure with two foundation forms at the same thickness of the rubber-improved soil layer. The maximum displacement of the frame structure with raft foundation at the same height observation point is smaller than the maximum displacement of the frame structure with strip foundation, indicating that increasing the contact area between the base and the rubber-improved soil isolation layer can effectively reduce the maximum displacement of the frame structure. And with the increase of the thickness of the rubber-improved soil isolation layer, the gap between the column height-absolute displacement curves of the two foundation forms increases, indicating that increasing the thickness of the rubber-improved soil isolation layer will make the contact area between the different bases and the rubber-improved soil isolation layer on the frame structure column height-absolute displacement more significant.
[0114] Table 3 Maximum displacement and maximum displacement difference of observation column in Examples 1 to 3 and Comparative Examples 1 to 5 Maximum displacement(m) Maximum displacement(m) Maximum displacement difference (m) Comparative Example 2 0.0374 Comparative Example 1 0.0364 0.0010 Comparative Example 3 0.0332 Example 1 0.0312 0.0020 Comparative Example 4 0.03 Example 2 0.0266 0.0034 Comparative Example 5 0.0278 Example 3 0.0238 0.0040 Further quantitative analysis is provided in Table 3: Under the premise of the same thickness of rubber-modified soil isolation layer, the maximum displacement of the frame structure with raft foundation is smaller than that of strip foundation. Under the premise of the same thickness of rubber-modified soil isolation layer, the maximum displacement difference between the two foundation forms increases with the increase of the thickness of rubber-modified soil isolation layer, indicating that increasing the thickness of rubber-modified soil isolation layer can increase the difference of base contact area on the isolation effect of frame structure.
[0115] An artificial seismic wave with an acceleration peak of 0.1g was selected as the dynamic load. The artificial seismic wave was a shear wave propagating vertically upward. The equivalent node force was applied to the two-layer frame structures of Examples 1 to 3 and Comparative Examples 1 to 5. An observation point was set every 1m on the observation column at the same position in the frame structures of Examples 1 to 3 and Comparative Examples 1 to 5. The maximum shear stress corresponding to each observation point was extracted to obtain a column height-maximum shear stress curve, as shown in FIG. Figure 3 shown.
[0116] Depend on Figure 3 Qualitative analysis of (a) to (d) shows that: The column height-maximum shear stress curves under the two foundation forms have the same trend of change, that is, the maximum shear stress decreases with the increase of height. And the maximum shear stress of the observed columns under the two foundation forms decreases with the increase of the thickness of the rubber-improved soil isolation layer, indicating that increasing the thickness of the rubber-improved soil layer can effectively reduce the maximum shear stress of the frame structure.
[0117] In the same thickness of rubber-modified soil isolation layer, the maximum shear stress of the raft foundation frame structure is smaller than that of the strip foundation frame structure, indicating that increasing the contact area between the base and the rubber-modified soil isolation layer can effectively reduce the maximum shear stress of the frame structure. As the thickness of the rubber-modified soil isolation layer increases, the distance between the column height-maximum shear stress curves between the two foundation forms also increases, indicating that increasing the thickness of the rubber-modified soil isolation layer can reduce the difference between the contact areas of different bases.
[0118] 2.2 Effect of thickness of rubber-modified soil isolation layer on isolation effect In order to study the shock-absorbing effect of the thickness of the rubber-modified soil isolation layer on the frame structure, an artificial seismic wave with an acceleration peak of 0.2g was selected as the dynamic load. The artificial seismic wave was a shear wave propagating vertically upward and was applied to the frame structures of Comparative Examples 1 to 5 and Examples 1 to 3 by using an equivalent nodal force input method. The peak value of the top acceleration of the observation column of the frame structure and the reduction amplitude (referred to as reduction amplitude) of the acceleration peak value of isolation layers of different thicknesses relative to no shock-absorbing layer (Comparative Example 1 or 2) under the same foundation form were obtained. The experimental test results are shown in Table 4.
[0119] Table 4 Peak acceleration and drop of the frame structure in Examples 1 to 3 and Comparative Examples 1 to 5 From Table 4, we can see that: Compared with Comparative Example 1, the acceleration peak reduction amplitudes of Examples 1 to 3 are 46.5%, 51.65% and 53.78% respectively, among which the acceleration peak reduction amplitude of Example 2 is increased by 5.15% compared with Example 1, and the acceleration peak reduction amplitude of Example 3 is increased by 2.13% compared with Example 2, which is not as significant as the former. Compared with Comparative Example 2, the variation pattern of Comparative Examples 3 to 5 is the same as that of Examples 1 to 3 relative to Comparative Example 1, but under the same thickness of rubber improved soil isolation, the shock absorption effect is always relatively small.
[0120] In order to study the effect of the rubber-modified soil isolation layer on the displacement of the frame structure, an observation point is set every 1m for the observation column mentioned above, and the maximum displacement of each observation point is extracted to form a column height-maximum displacement curve. An artificial seismic wave with an acceleration peak of 0.2g is selected as the dynamic load. The artificial seismic wave is a shear wave that propagates vertically upward. The equivalent node force is applied to the two-story frame structure of Examples 1 to 3 and Comparative Example 1 to obtain a column height-absolute displacement peak curve, as shown in the figure. Figure 4 shown.
[0121] Depend on Figure 4 It can be seen that although the thickness of the rubber-modified soil seismic isolation layer in Examples 1 to 3 and Comparative Example 1 is different, the change trends of the column height-maximum displacement curves are consistent, that is, the displacement increases with the increase of height.
[0122] With the increase of the thickness of the rubber-improved soil isolation layer, the lateral horizontal displacement at the same height gradually decreases, and when the thickness of the rubber-improved soil isolation layer is less than 0.6m, the lateral horizontal displacement of the frame structure decreases significantly, and when the thickness of the rubber-improved soil isolation layer is greater than or equal to 0.6m, the lateral horizontal displacement of the frame structure decreases slightly, indicating that increasing the thickness of the rubber-improved soil isolation layer can effectively reduce the lateral horizontal displacement of the frame structure. When the thickness of the rubber-improved soil isolation layer reaches 0.6m, the shock-absorbing effect is close to the limit, and continuing to increase the thickness of the rubber-improved soil isolation layer will reduce the lateral horizontal displacement of the frame structure slightly.
[0123] In order to obtain an intuitive description of the displacement limit of the structure under earthquake action, the present application proposes the calculation of the displacement angle of the structure. The structural limit displacement is now described by calculating the displacement angle of the column in the structure. The calculation of the displacement angle of the column is shown below. The maximum displacement angle of each observed column in Examples 1 to 3 and Comparative Example 1 is shown in Table 5. Displacement angle = 100% × horizontal displacement of the top of the component / component height Table 5 shows the maximum displacement angles of the frame structure observation columns in Examples 1 to 3 and Comparative Example 1 Comparative Example 1 Example 1 Example 2 Example 3 Displacement angle (%) 0.61 0.468 0.423 0.415 By analyzing the maximum displacement angle of the observation column of the frame structure in Examples 1 to 3 and Comparative Example 1, it can be concluded that the displacement angle of the frame structure in Comparative Example 1 and Example 1 has decreased significantly, indicating that the rubber-modified soil isolation layer can effectively reduce the displacement angle isolation effect of the frame structure, and the rubber-modified soil layer can effectively block the displacement response of the frame structure under earthquake action, reducing the displacement of the frame structure under earthquake action. The reduction of the displacement angle in Examples 2 and 3 also has a significant effect, but the difference in isolation effect between the two is very small. It can be concluded that the thickness of the rubber particle-modified soil isolation layer is 0.6m, which is the best solution.
[0124] 2.3 Impact of ground motion intensity on seismic isolation effect An artificial seismic wave is selected as the dynamic load, and the peak acceleration is adjusted to 0.1g, 0.2g and 0.4g respectively. The artificial seismic wave is a shear wave that propagates vertically upward. It is applied to the frame structures of Comparative Example 1 and Example 1 by inputting an equivalent nodal force. The peak acceleration of the observed column vertices of the frame structures of Example 1 and Comparative Example 1 under different seismic motion intensities are obtained. The results are shown in Table 6.
[0125] Table 6 Peak acceleration of the observation column vertex of the frame structure of Example 1 and Comparative Example 1 under different earthquake intensities Further quantitative analysis is performed from Table 6: the vertex acceleration of the frame structure of Comparative Example 1 and Example 1 increases with the increase of the input seismic motion intensity. When the input seismic wave intensity is 0.1g, 0.2g and 0.4g, the vertex acceleration peak value of the frame structure of Example 1 is reduced by 16.97%, 46.5% and 51.03% respectively compared with the frame structure of Comparative Example 1, and the reduction amplitude of the vertex acceleration increases with the increase of the seismic wave intensity, indicating that the shock absorption effect of Example 1 (i.e., laying the rubber improved soil isolation layer) is better as the seismic wave intensity increases.
[0126] Artificial seismic waves were selected as dynamic loads, and the peak accelerations were adjusted to 0.1g, 0.2g and 0.4g respectively. The artificial seismic waves were shear waves that propagated vertically upward. An observation point was set every 1m for the observation column mentioned above. The equivalent nodal force was applied to the frame structures of Comparative Example 1 and Example 1 by inputting the force. The maximum displacement and the maximum shear stress of the observation column in Comparative Example 1 and Example 1 were recorded under different seismic intensities. The results are shown in Tables 7-8.
[0127] Table 7 Maximum displacement of the observation column in Comparative Example 1 and Example 1 Artificial seismic wave intensity Comparative Example 1 Maximum displacement (m) Example 1 Maximum displacement (m) Decrease (%) 0.1g 0.0364 0.0312 14.28 0.2g 0.0423 0.0356 15.83 0.4g 0.0485 0.0403 16.9 Table 8 Maximum shear stress of the observation column in Comparative Example 1 and Example 1 Artificial seismic wave intensity Comparative Example 1 Maximum shear stress (Pa) Example 1 Maximum shear stress (Pa) Decrease (%) 0.1g 22765 21674 4.79 0.2g 26694 22348 16.28 0.4g 32267 26549 17.72 It can be seen from Tables 7 and 8 that when the peak value of the input artificial seismic wave acceleration is 0.1g, 0.2g and 0.4g, the maximum displacement of the observation column of the frame structure of Example 1 is reduced by 14.28%, 15.83% and 16.9% respectively compared with the maximum displacement of the observation column of the frame structure of Comparative Example 1, and the maximum shear stress reduction of the observation columns of the two is gradually increased by 4.79%, 16.28% and 17.72% respectively, indicating that as the peak value of the seismic wave acceleration increases, the shock absorption effect of the frame structure of Example 1 (i.e., laying the rubber particle improved soil isolation layer) is enhanced.
[0128] 2.4 Impact of ground motion spectrum characteristics on seismic isolation effect Friuli seismic waves, San Fernando seismic waves and artificial seismic waves were selected, and the acceleration peaks of the above three seismic waves were set to 0.2g, and were respectively input into the frame structures of Example 2 and Comparative Example 1, and the Fourier spectra of Example 2 and Comparative Example 1 under the action of different types of seismic waves were obtained, as shown in FIG. Figure 5 .
[0129] Depend on Figure 5 It can be seen that the Fourier spectra of Example 2 and Comparative Example 1 are basically consistent with the input seismic Fourier spectrum curve shape, and there is a difference between the Fourier curve shape of the input artificial seismic wave and the Fourier spectra of Example 2 and Comparative Example 1. This is because the frame structure of Comparative Example 1 has a more severe structural reaction during an earthquake than the frame structure of Example 1, internal damage and deformation continue to accumulate and cracks are generated, and the natural frequency is reduced.
[0130] Under the action of different types of seismic waves, the basic frequencies of the Fourier spectra corresponding to the acceleration time history of the frame structure vertices are close, but the Fourier amplitudes corresponding to the basic frequencies show certain differences, that is, the Fourier amplitudes under the action of artificial waves are higher than the corresponding values under the action of Friuli waves and San Fernando waves. This may be because the low-frequency components of artificial waves are richer, resulting in a more intense dynamic response of the frame structure; the amplitudes of the Fourier spectra of the structural response and the input seismic Fourier spectrum under the action of the three seismic waves are reduced. This is because the rubber-modified soil isolation layer in Example 1 makes the soil-structure interaction smoother, the nonlinear residual deformation of the soil is weak, and the amplitude corresponding to the basic frequency is reduced.
[0131] 2.5 An artificial seismic wave is selected as the dynamic load, and the peak acceleration is adjusted to 0.1g. The artificial seismic wave is a shear wave propagating vertically upward. An observation point is set every 1m for the observation column mentioned above, and the equivalent node force is applied to the frame structures of Examples 1 to 17 and Comparative Examples 1 to 5. The maximum displacement of the observation column, the peak acceleration of the observation column, and the maximum shear stress of the observation column in Comparative Example 1 and Example 1 are recorded under different seismic intensities. The results are shown in Table 9.
[0132] Table 9 Maximum shear stress, maximum displacement and peak acceleration of the frame structure of Examples 1 to 17 and Comparative Examples 1 to 5 It can be seen from Table 9 that, by comparing and analyzing Examples 1 to 3 and Comparative Example 1, the rubber-modified soil isolation layer has a better isolation effect, and by increasing the thickness of the rubber-modified soil isolation layer, the isolation effect of the frame structure is gradually increased.
[0133] By comparing and analyzing Examples 2 to 9, it can be seen that by adjusting the ratio of fulvic acid solution, mixed solution A, and mixed solution B in the rubber-improved soil, and gradually modifying the quicklime and introducing a curing agent, the curing effect and compressive strength of the rubber-improved soil layer can be improved, thereby enhancing the seismic isolation effect of the frame structure. This is mainly because the modified quicklime can enhance the capture of carbon dioxide, and its adsorption properties are mainly reflected in solid-phase physical adsorption and liquid-phase chemical absorption, so that more calcium carbonate precipitation can be generated in the soil, making the compressive strength of the rubber-improved soil layer higher. The curing agent can also further work together with fly ash to condense and dehydrate the surface hydroxyl groups between different silicon oxygen chains, produce cross-linking, and further solidify the soil.
[0134] By comparing and analyzing Examples 10 to 15, by further setting inverted cone pits arranged in a matrix below the rubber-modified soil isolation layer and modifying the rubber particles, the intensity of the upward propagation of seismic waves is weakened, and the bonding force between the rubber particles and the surrounding soil particles is enhanced, thereby further enhancing the isolation effect.
[0135] By comparing and analyzing Examples 16 to 18, it can be seen that by optimizing the raw soil, fly ash, rubber particles and quicklime powder in the rubber-improved soil, when the volume of the rubber particles accounts for about 30%, the seismic isolation effect of the rubber-improved soil isolation layer is better.
Claims
1. A construction method for a rubber-modified soil seismic isolation layer for a frame structure, characterized in that: The steps include: S1: Excavate the foundation pit according to the normal construction process, and the depth should not be less than that of the ordinary foundation pit; S2: Backfill the foundation pit soil at the bottom of the foundation pit, then lay and compact the rubber improved soil, cover and maintain for 2 to 4 days to obtain the rubber improved soil seismic isolation layer; S3: A raft foundation is set above the rubber improved soil isolation layer, and a frame structure is set on the raft foundation; The rubber improved soil comprises foundation pit soil, rubber particles, fly ash, quicklime, ferrous sulfate, hydrogen peroxide, citric acid, sodium citrate, fulvic acid and water.
2. The construction method of the rubber improved soil seismic isolation layer for frame structure according to claim 1 is characterized in that: The method for preparing the rubber-improved soil comprises the following steps: The foundation pit soil is dried and crushed to obtain raw soil, and the raw soil, fly ash and rubber particles are evenly mixed to obtain mixed soil; After the humic acid solution, the mixed solution A, the mixed solution B and the mixed soil are mixed evenly, quicklime is added and mixed evenly to obtain rubber-improved soil; The fulvic acid solution comprises fulvic acid and water; The mixed solution A comprises ferrous sulfate, citric acid and water; The mixed solution B includes hydrogen peroxide, citric acid-sodium citrate and water.
3. The construction method of the rubber improved soil seismic isolation layer for frame structure according to claim 2 is characterized in that: The volume ratio of the raw materials soil, fly ash, quicklime and rubber particles is 6-10:1.5-3.5:0.1-0.2:2-7.
4. The construction method of the rubber improved soil seismic isolation layer for frame structure according to claim 3 is characterized in that: The quicklime is modified quicklime, and the preparation method of the modified quicklime comprises the following steps: The biochar, sodium hydroxide and water are mixed evenly, allowed to stand and soak, quicklime is added and mixed evenly, the solid and liquid are separated, washed and dried, sintered at 500-600°C for 2-4 hours, cooled and crushed to obtain modified quicklime.
5. The construction method of the rubber improved soil seismic isolation layer for frame structure according to claim 4, characterized in that: The mass ratio of the biochar to quicklime is 1:2-5.
6. The construction method of the rubber improved soil seismic isolation layer for frame structure according to claim 5, characterized in that: In step 2), a curing agent is also added to the fulvic acid solution, and the preparation method of the curing agent comprises the following steps: After monomer A, monomer B, 1-butene, polymerization inhibitor and water are mixed evenly, initiator is added and mixed evenly, the temperature is raised to 60-80°C, reacted for 4-6 hours, solid-liquid separation is performed, and dried to obtain a curing agent; The monomer A is at least one of methacrylic acid and 2-ethylacrylic acid; The monomer B is at least one of sodium methyl propylene sulfonate and sodium allyl sulfonate.
7. The construction method of a rubber-modified soil seismic isolation layer for a frame structure according to claim 6, characterized in that: In step S2, after partially backfilling the foundation pit soil at the bottom of the foundation pit, a foundation pit soil layer is obtained, and inverted cone holes arranged in a matrix are excavated at intervals on the foundation pit soil layer, and the inverted cone holes are filled and compacted with foundation improved soil, and then the rubber improved soil is laid and compacted; The foundation improved soil comprises foundation pit soil, rubber particles, calcium chloride, water glass, polyacrylamide and water.
8. The construction method of a rubber-modified soil seismic isolation layer for a frame structure according to claim 7, characterized in that: The method for preparing the basic improved soil comprises the following steps: The foundation pit soil is dried and crushed to obtain raw soil, the raw soil and rubber particles accounting for 40-60% of the total volume of the raw soil and rubber particles are evenly mixed, and then the mixed liquid is added and mixed evenly to obtain foundation improved soil; The mixed solution is a mixed solution of calcium chloride, water glass, polyacrylamide and water.
9. The construction method of the rubber improved soil seismic isolation layer for frame structure according to claim 8, characterized in that: The rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps: The rubber particles are mixed evenly with the alkali solution, left to stand for 18 to 24 hours, separated from the solid and the liquid, washed, mixed evenly with the silane coupling agent, silicone resin and water, then added with water glass, mixed evenly, separated from the solid and the liquid, and dried to obtain modified rubber particles.
10. The construction method of the rubber improved soil seismic isolation layer for frame structure according to claim 9, characterized in that: In step S2, after the maintenance of the rubber improved soil isolation layer is completed, the rubber improved soil isolation layer is sprayed with 10-20L / m 2 After spraying the alkali solution, leave it for 1 to 3 days.