Method for detecting total silicon, total aluminum and total titanium in steel and cast iron

Through inductively coupled plasma atomic emission spectroscopy (ICP-AES) combined with nitric acid-hydrochloric acid dissolution and mixed flux melting treatment, the problem of low detection results of all titanium, all silicon and all aluminum in cast iron and steel in the prior art is solved. Accurate determination of these elements is achieved, meeting customers' precise control requirements for chemical elements.

CN118758922AInactive Publication Date: 2024-10-11BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410664932.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art detects acid insoluble in conventional testing when detecting all titanium, all silicon and all aluminum in cast iron and steel, resulting in low results and cannot meet customers' precise control requirements for chemical elements.

Method used

Inductively coupled plasma atomic emission spectroscopy (ICP-AES) was used to weigh the samples and dissolve, filtration and precipitate the samples, melt them using mixed flux, and introduce them to the spectrometer for measurement after filtrate leaching, combining with known concentration standard substances. The working curve outputs element concentration. The specific steps include dissolving the sample with mixed acid, heating it to dissolve at a low temperature, filtration, adding mixed flux to melt, and measuring the spectral line intensity of the element to be measured.

Benefits of technology

It realizes the accurate determination of the content of all titanium, all silicon and all aluminum in cast iron and steel, meets customers' strict requirements for chemical elements, provides an effective and practical detection method, and improves the detection accuracy and precision.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004860802290000041
    Figure BDA0004860802290000041
Patent Text Reader

Abstract

The invention discloses a method for detecting total silicon, total aluminum and total titanium in steel and cast iron, which comprises the following steps: weighing a certain amount of sample, dissolving the sample with nitric acid-hydrochloric acid, filtering, melting the precipitate with a mixed flux, leaching the filtrate, transferring into a volumetric flask, diluting to a certain volume, atomizing the solution, introducing into an inductively coupled plasma atomic emission spectrometer, and measuring the total silicon, total aluminum and total titanium in the steel and cast iron. And measuring the intensity of the spectral line of the to-be-measured element. And finally, outputting the concentration of the corresponding element in the substance to be detected according to the working curve of the standard substance with known concentration. In order to control the quality of cast iron and steel products, the invention aims to provide the method for detecting all silicon, all aluminum and all titanium in steel and cast iron, and the method is used for production practice and is an effective and practical method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgical analysis, and in particular to a method for detecting full silicon, full aluminum and full titanium in steel and cast iron. Background Art

[0002] With the development of internationalization of the steel industry, increasingly stringent requirements have been put forward for cast iron and steel materials. In addition to the requirements for the mechanical properties of materials, various chemical compositions that affect material performance and environmental safety are also required to be precisely controlled. The national standard "Spheroidal Graphite Castings" has no requirements for chemical composition, but some foreign customers have strict requirements and stipulate that more than 20 chemical elements need to be controlled for ductile iron. Silicon can improve the strength and local corrosion resistance in ordinary low-alloy steel, and is one of the main alloys in alloy structure. In stainless steel and corrosion-resistant steel, silicon can be combined with aluminum, titanium, nitrogen and other elements to improve corrosion resistance and high-temperature oxidation resistance. Inductively coupled plasma optical emission spectroscopy (ICP-OES) has high sensitivity, low interference, low detection limit, and can simultaneously determine multiple elements. It has been widely used in various fields of analysis and detection. Titanium, silicon and aluminum are insoluble in acid in conventional detection, resulting in low results in conventional detection. Based on the above situation, we have invented a method for detecting the content of all titanium, all silicon and all aluminum in cast iron and steel. Summary of the invention

[0003] In order to control the quality of cast iron and steel products, the purpose of the present invention is to provide a method for detecting full silicon, full aluminum and full titanium in steel and cast iron. This method has been used in production practice and is an effective and practical method.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention discloses a method for detecting full silicon, full aluminum and full titanium in steel and cast iron, comprising the following steps:

[0006] Weigh a certain amount of sample, dissolve it with nitric acid-hydrochloric acid, filter it, melt the precipitate with mixed flux, extract the filtrate, transfer it to a volumetric flask and dilute it to a certain volume, atomize the solution and introduce it into the inductively coupled plasma atomic emission spectrometer to measure the intensity of the spectral line of the element to be tested. Finally, output the concentration of the corresponding element in the substance to be tested through the working curve of the known concentration standard substance.

[0007] Further, 0.2000 g of the sample was weighed, placed in a 250 mL beaker, 30 mL of mixed acid was added, heated at low temperature until the sample was completely dissolved and cooled to room temperature, filtered with medium-speed quantitative filter paper, and the filtrate was transferred to a beaker; the beaker was washed with hydrochloric acid for 3 times, and the precipitate was washed 7-8 times; the precipitate was washed with water for 4-5 times, the precipitate and the filter paper were transferred to a platinum crucible, ashed, 0.50 g of mixed flux was accurately added, and the mixture was melted in a high-temperature furnace at 900 ° C for 8 minutes, the filtrate was leached with the filtrate, and the molten block was transferred to a 100 mL plastic volumetric flask, made up to volume with water, and shaken well; and the machine was tested.

[0008] Furthermore, the measurement ranges are: Al: 0.001% to 2.00%; Ti: 0.001% to 2.50%; Si: 0.030% to 3.00%.

[0009] Furthermore, the mixed acid includes hydrochloric acid, nitric acid and water in a volume ratio of 1:1:3.

[0010] Furthermore, the OPTIMA 5300DV bidirectional observation full spectrum direct reading plasma spectrometer produced by PE Company of the United States was used for detection.

[0011] Furthermore, the mixed flux is specifically anhydrous sodium carbonate and boric acid / anhydrous sodium tetraborate, with a mass ratio of 2:1.

[0012] Compared with the prior art, the beneficial technical effects of the present invention are:

[0013] Accurate analysis of the content of chemical elements in cast iron and steel is an important means to control the quality of later steel products. To this end, the present invention provides a method for detecting the content of all titanium, all silicon and all aluminum in cast iron and steel. This method has been used in production practice, and the measurement results are accurate. It is an effective and practical method that can be promoted and applied in the metallurgical industry and related scientific research institutes. DETAILED DESCRIPTION

[0014] A method for detecting full silicon, full aluminum, and full titanium in steel and cast iron, comprising:

[0015] 1 Scope

[0016] This method specifies the use of I CP-AES to simultaneously determine the total titanium, total silicon and total aluminum content in cast iron and steel.

[0017] Measurement range: Al: 0.001% ~ 2.00%; Ti: 0.001% ~ 2.50%; Si: 0.030% ~ 3.00%.

[0018] 2 Method Summary

[0019] Weigh a certain amount of sample, dissolve it with nitric acid-hydrochloric acid, filter it, melt the precipitate with mixed flux, extract the filtrate, transfer it to a volumetric flask and dilute it to a certain volume, atomize the solution and introduce it into the inductively coupled plasma atomic emission spectrometer to measure the intensity of the spectral line of the element to be tested. Finally, output the concentration of the corresponding element in the substance to be tested through the working curve of the known concentration standard substance.

[0020] 3 Reagents and materials

[0021] 3.1 High purity iron powder

[0022] 3.2 Anhydrous sodium carbonate

[0023] 3.3 Boric acid

[0024] 3.4 Hydrochloric acid, ρ about 1.19 g / mL

[0025] 3.5 Nitric acid, ρ about 1.42 g / mL

[0026] 3.6 Titanium, silicon, aluminum standard solution, 1000 μg / mL

[0027] 3.7 Anhydrous sodium tetraborate

[0028] 4. Main instruments and test conditions

[0029] 4.1 Produced by PE Company of the United States, OPTI MA 5300DV two-way observation full spectrum direct reading plasma spectrometer has multi-spectrum fitting function.

[0030] 4.2 Instrument parameters: see the table below

[0031] Working parameter table

[0032]

[0033] 4.3 The wavelengths of the analytical lines of the elements to be measured are: titanium 334.941nm silicon 251.611nm aluminum 396.152nm

[0034] 5 Analysis steps

[0035] 5.1 Sample quantity

[0036] Weigh 0.2000g of sample, accurate to 0.0002g.

[0037] 5.2 Determination steps

[0038] Place the weighed sample in a 250mL beaker, add 30mL of mixed acid (1+1+3), heat at low temperature until the sample is completely dissolved and cool to room temperature, filter with medium-speed quantitative filter paper, and transfer the filtrate to a beaker. Wash the beaker 3 times with hydrochloric acid (5+95), and wash the precipitate 7-8 times. Wash the precipitate 4-5 times with water, transfer the precipitate and the filter paper into a platinum crucible, ash, accurately add 0.50g of mixed flux, melt in a 900℃ high-temperature furnace for 8 minutes, use the filtrate to extract the molten block, transfer it to a 100mL plastic volumetric flask, make up to volume with water, and shake well. Test on the machine.

[0039] 5.3 Curve drawing

[0040] Weigh high-purity iron corresponding to the measured cast iron and steel in 6 beakers as the matrix and add the corresponding mixed flux, add mixed acid to dissolve, cool to room temperature, transfer to 100mL volumetric flasks respectively, and then transfer the standard solution to the volumetric flask as needed, dilute with water to the scale and shake well, and draw a curve according to the content value of each element.

[0041] 6 Results and discussion

[0042] 6.1 Accuracy Experiment

[0043] Weigh cast iron and steel standard samples respectively, and conduct testing experiments according to this method. The results are shown in Table 1:

[0044] Table 1 Accuracy of measurement results (%)

[0045] Elements to be measured Cast iron test value Cast iron value Alloy steel test value Alloy steel value <![CDATA[Ti t ]]> 0.055 0.056 0.0026 0.0028 <![CDATA[Si t ]]> 2.27 2.28 0.294 0.293 <![CDATA[Al t ]]> 0.011 0.011 0.037 0.037

[0046] It can be seen from the data in the table that the detection method has high accuracy.

[0047] 6.2 Precision experiment

[0048] Weigh 11 standard samples of alloy steel and perform precision tests according to the above experimental method. The test results are shown in Table 2:

[0049] Table 2 Determination results precision table (%)

[0050] Elements to be measured average value Standard Deviation RSD <![CDATA[Ti t ]]> 0.033 0.10% 1.23% <![CDATA[Si t ]]> 0.255 0.11% 1.37% <![CDATA[Al t ]]> 0.030 0.12% 1.34%

[0051] The above data show that the detection method has good precision.

[0052] 7 Conclusion

[0053] The method can accurately determine the content of all titanium, all silicon and all aluminum in cast iron and steel. The method is simple to operate and easy to master, and can meet production needs.

[0054] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for detecting full silicon, full aluminum, and full titanium in steel and cast iron, characterized by: The following steps are involved: Weigh a certain amount of sample, dissolve it with nitric acid-hydrochloric acid, filter it, melt the precipitate with mixed flux, extract the filtrate, transfer it to a volumetric flask and dilute it to a certain volume, atomize the solution and introduce it into the inductively coupled plasma atomic emission spectrometer to measure the intensity of the spectral line of the element to be tested. Finally, output the concentration of the corresponding element in the substance to be tested through the working curve of the known concentration standard substance.

2. The method for detecting full silicon, full aluminum and full titanium in steel and cast iron according to claim 1, characterized in that: Weigh 0.2000g of the sample, place the weighed sample in a 250mL beaker, add 30mL of mixed acid, heat at low temperature until the sample is completely dissolved and cool to room temperature, filter with medium-speed quantitative filter paper, and transfer the filtrate to a beaker; wash the beaker 3 times with hydrochloric acid, wash the precipitate 7-8 times; wash the precipitate 4-5 times with water, transfer the precipitate and the filter paper into a platinum crucible, ashed, accurately add 0.50g of mixed flux, melt in a 900℃ high-temperature furnace for 8min, soak the fused block with the filtrate, transfer it to a 100mL plastic volumetric flask, make up to volume with water, shake well, and test on the machine.

3. The method for detecting full silicon, full aluminum and full titanium in steel and cast iron according to claim 2, characterized in that: Measurement range: Al: 0.001% ~ 2.00%; Ti: 0.001% ~ 2.50%; Si: 0.030% ~ 3.00%.

4. The method for detecting full silicon, full aluminum and full titanium in steel and cast iron according to claim 2, characterized in that: The mixed acid is hydrochloric acid, nitric acid and water; the volume ratio is 1:1:

3.

5. The method for detecting full silicon, full aluminum and full titanium in steel and cast iron according to claim 2, characterized in that: The OPTIMA 5300DV bidirectional observation full spectrum direct reading plasma spectrometer produced by PE Company of the United States was used for detection.

6. The method for detecting full silicon, full aluminum and full titanium in steel and cast iron according to claim 1, characterized in that: The mixed solvent includes anhydrous sodium carbonate, boric acid or anhydrous sodium tetraborate in a mass ratio of 2:1.

Citation Information

Patent Citations

  • Determination method of total aluminum content in steel and alloy

    CN103698176A

  • Method for determining the total aluminum content in steel by using an inductively coupled plasma atomic emission spectrometer

    CN108120711A