Display panel and manufacturing method thereof

By using flexible frame glue in the display panel, the probability of water vapor intrusion is reduced, the adverse phenomena caused by water vapor intrusion in the display panel are solved, and its stability and water-blocking performance are improved.

CN118759748APending Publication Date: 2024-10-11GUANGZHOU CHINA STAR OPTOELECTRONICS SEMICON DISPLAY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410884001.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-11

Smart Images

  • Figure CN118759748A_ABST
    Figure CN118759748A_ABST
Patent Text Reader

Abstract

The invention discloses a display panel and a manufacturing method thereof. The display panel comprises a first substrate, a second substrate, liquid crystal and frame glue. The first substrate and the second substrate are oppositely arranged; the frame glue is connected between the first substrate and the second substrate; the liquid crystal is arranged in a space enclosed by the first substrate, the second substrate and the frame glue; wherein the frame glue comprises an epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%; according to the display panel and the display device, the probability that microcracks appear at the connecting interface of the frame glue and the substrate can be effectively reduced, the probability that water vapor invades into the display panel from the connecting interface of the frame glue and the substrate is reduced, the water blocking performance of the display panel is improved, the probability that the display panel generates undesirable phenomena due to water vapor invasion is reduced, and the display quality is improved. And the stability of the display panel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of display technology, and in particular to a display panel and a manufacturing method thereof. Background Art

[0002] Consumers have increasingly higher requirements for display panels, which is reflected not only in the increasing requirements for optical specifications in the conventional sense, but also in the increasing requirements for the reliability specifications of display panels.

[0003] Currently, during the transportation and use of the display panel, water vapor easily intrudes into the interior of the display panel, causing poor display effects on the display panel, for example, causing the display panel to be black. Summary of the invention

[0004] The embodiments of the present application provide a display panel and a method for manufacturing the same, which can reduce the probability of adverse phenomena occurring in the display panel due to water vapor intrusion and improve the stability of the display panel.

[0005] An embodiment of the present application provides a display panel, comprising:

[0006] a first substrate;

[0007] a second substrate, arranged opposite to the first substrate;

[0008] A frame glue connected between the first substrate and the second substrate; and

[0009] Liquid crystal is arranged in a space enclosed by the first substrate, the second substrate and the frame glue;

[0010] The sealant includes epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%.

[0011] In one embodiment of the present application, the curing rate of the epoxy resin polymer is greater than or equal to 40%.

[0012] In one embodiment of the present application, the curing rate of the epoxy resin polymer is lower than the curing rate of the acrylic.

[0013] In one embodiment of the present application, the curing rate of the acrylic is greater than or equal to 85% and less than or equal to 92%.

[0014] In one embodiment of the present application, the elastic modulus of the sealant is greater than or equal to 3.1 GPa and less than or equal to 3.4 GPa.

[0015] In one embodiment of the present application, the moisture permeability of the sealant is less than or equal to 57 g / m 2 .

[0016] According to the above-mentioned purpose of the present application, an embodiment of the present application further provides a method for manufacturing a display panel, which comprises the following steps:

[0017] forming a sealant intermediate on the first substrate;

[0018] Disposing liquid crystal on the first substrate, wherein the liquid crystal is located in the area enclosed by the frame glue intermediate;

[0019] Disposing a second substrate on the first substrate;

[0020] The sealant intermediate connected between the first substrate and the second substrate is cured, wherein the sealant formed after the sealant intermediate is cured includes epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%.

[0021] In one embodiment of the present application, the sealant intermediate includes acrylic small molecules, epoxy resin, photoinitiator and thermal initiator;

[0022] The curing process of the sealant intermediate connected between the first substrate and the second substrate includes:

[0023] Performing a light-curing treatment on the sealant intermediate to polymerize at least a portion of the acrylic small molecules;

[0024] The sealant intermediate is subjected to a heat curing treatment, and a portion of the epoxy resin is polymerized.

[0025] In one embodiment of the present application, the temperature of the thermal curing treatment is less than or equal to 120° C., and the duration of the thermal curing treatment is less than 50 minutes.

[0026] In one embodiment of the present application, in the step of curing the frame glue intermediate connected between the first substrate and the second substrate, the curing rate of the epoxy resin polymer is greater than or equal to 40%, and the curing rate of the acrylic is greater than or equal to 85% and less than or equal to 92%.

[0027] Beneficial effects of the present application: The present application can reduce the curing rate of the epoxy resin polymer in the frame glue, thereby reducing the elastic modulus of the frame glue and increasing the flexibility of the frame glue, thereby effectively reducing the probability of microcracks appearing at the connection interface between the frame glue and the substrate, reducing the probability of water vapor intruding into the display panel from the connection interface between the frame glue and the substrate, improving the water-blocking performance of the display panel, reducing the probability of adverse phenomena occurring in the display panel due to water vapor intrusion, and improving the stability of the display panel. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1A schematic diagram of a structure of a display panel provided in an embodiment of the present application;

[0029] Figure 2 A schematic diagram of a force direction of a display panel provided in an embodiment of the present application;

[0030] Figure 3 A schematic diagram of another force direction of a display panel provided in an embodiment of the present application;

[0031] Figure 4 A schematic diagram of another structure of a display panel provided in an embodiment of the present application;

[0032] Figure 5 A flow chart of a method for manufacturing a display panel provided in an embodiment of the present application. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application.

[0034] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the various specific processes and material examples provided by the present application, but those of ordinary skill in the art can appreciate the application of other processes and / or the use of other materials.

[0035] An embodiment of the present application provides a display panel 10 , which includes a first substrate 11 , a second substrate 12 , a liquid crystal 41 , and a sealant 20 .

[0036] The first substrate 11 and the second substrate 12 are arranged opposite to each other, the frame glue 20 is connected between the first substrate 11 and the second substrate 12 , and the liquid crystal 41 is arranged in a space enclosed by the first substrate 11 , the second substrate 12 and the frame glue 20 .

[0037] The sealant 20 includes epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%.

[0038] During the implementation of the application, the present application can reduce the curing rate of the epoxy resin polymer in the frame glue 20, thereby reducing the elastic modulus of the frame glue 20 and increasing the flexibility of the frame glue 20, thereby effectively reducing the probability of microcracks appearing at the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12, and reducing the probability of the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12 invading the display panel 10, thereby improving the water-blocking performance of the display panel 10, reducing the probability of adverse phenomena caused by water vapor intrusion in the display panel 10, and improving the stability of the display panel 10.

[0039] In some embodiments, the display panel 10 includes the first substrate 11 and the second substrate 12 arranged relatively to each other, a frame glue 20 arranged between the first substrate 11 and the second substrate 12, a liquid crystal 41 arranged between the first substrate 11 and the second substrate 12, and a first polarizer 31 and a second polarizer 32 respectively arranged on the first substrate 11 and the second substrate 12.

[0040] In some embodiments, the frame glue 20 is connected between the first substrate 11 and the second substrate 12, and the frame glue 20 is connected to the peripheral sides of the first substrate 11 and the second substrate 12 to enclose a space between the first substrate 11 and the second substrate 12, and the liquid crystal 41 is disposed in the space.

[0041] In some embodiments, the first polarizer 31 is disposed on a side of the first substrate 11 away from the second substrate 12 , and the second polarizer 32 is disposed on a side of the second substrate 12 away from the first substrate 11 .

[0042] It should be noted that the sealant 20 is bonded between the first substrate 11 and the second substrate 12, and can encapsulate, protect and block water in the area between the first substrate 11 and the second substrate 12; Figure 1 , Figure 2 as well as Figure 3 The display panel 10 is susceptible to stress during use or manufacturing. For example, when the first polarizer 31 and the second polarizer 32 shrink due to heat, the first substrate 11 and the second substrate 12 will also shrink and deform, thereby causing the sealant 20 connected between the first substrate 11 and the second substrate 12 to move, squeeze, deform, twist, and other undesirable phenomena. It is easy to generate microcracks at the interface between the sealant 20 and the first substrate 11 and the second substrate 12, so that water vapor invades the interior of the display panel 10 through the microcracks, resulting in display quality problems such as a black screen on the display panel 10.

[0043] The frame glue 20 includes an epoxy resin polymer and acrylic, and the frame glue 20 can be obtained by polymerizing epoxy resin and acrylic, and in an embodiment of the present application, the curing rate of the epoxy resin polymer in the frame glue 20 is less than or equal to 50%; that is, the embodiment of the present application can reduce the curing rate of the epoxy resin polymer, thereby reducing the elastic modulus of the frame glue 20 and increasing the flexibility of the frame glue 20, thereby effectively reducing the probability of microcracks appearing at the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12, reducing the probability of the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12 invading the display panel 10, improving the water-blocking performance of the display panel 10, reducing the probability of adverse phenomena caused by water vapor intrusion in the display panel 10, and improving the stability of the display panel 10.

[0044] In some embodiments, the curing rate of the epoxy resin polymer is greater than or equal to 40%, for example, it can be 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%; the embodiments of the present application need to maintain the mechanical strength of the frame glue 20 while improving the flexibility of the frame glue 20. Therefore, the curing rate of the epoxy resin polymer also needs to be greater than or equal to 40% to avoid the frame glue 20 being unable to stably connect between the first substrate 11 and the second substrate 12 due to insufficient mechanical strength.

[0045] In some embodiments, the curing rate of the epoxy resin polymer is less than the curing rate of the acrylic. Since the curing rate of the epoxy resin has been reduced in the embodiments of the present application, in order to ensure the mechanical strength and stability of the frame glue 20, the curing rate of the acrylic will at least be maintained from decreasing in the embodiments of the present application; wherein, the curing rate of the acrylic is greater than or equal to 85% and less than or equal to 92%, for example, it can be 85%, 86%, 87%, 88%, 89%, 90%, 91% or 92%.

[0046] It should be noted that the raw material components of the frame glue 20 include epoxy resin, acrylic small molecules, photoinitiator and thermal initiator. The embodiment of the present application improves the flexibility of the frame glue 20 by reducing the curing rate of the epoxy resin polymer, but does not improve the flexibility of the frame glue 20 by reducing the curing rate of the acrylic. Because the curing process of the frame glue 20 generally includes two stages of photocuring and thermal curing, wherein the acrylic small molecules undergo polymerization reaction mainly in the photocuring stage. The present application has been verified to find that if the curing rate of the acrylic small molecules is reduced, the photoinitiator will be precipitated, which will further contaminate the liquid crystal 41. Therefore, in the embodiment of the present application, by making the acrylic have a larger curing rate and reducing the curing rate of the epoxy resin, the precipitation of the photoinitiator can be effectively reduced, and the probability of the liquid crystal 41 being contaminated can be reduced. On this basis, the flexibility of the frame glue 20 can be increased, and the probability of microcracks generated at the interface between the frame glue 20 and the first substrate 11 and the second substrate 12 can be reduced, and the probability of water vapor invading the display panel 10 can be reduced.

[0047] In some embodiments, the epoxy resin can be one or a combination of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol H epoxy resin, novolac epoxy resin, multifunctional glycidyl ether epoxy resin, multifunctional glycidyl amine epoxy resin and halogenated epoxy resin.

[0048] In some embodiments, the elastic modulus of the sealant 20 is greater than or equal to 3.1 GPa and less than or equal to 3.4 GPa, for example, it may be 3.1 GPa, 3.2 GPa, 3.3 GPa or 3.4 GPa.

[0049] In some embodiments, the moisture permeability of the sealant 20 is less than or equal to 57 g / m 2 It should be noted that the moisture permeability of the sealant 20 at 85°C and 85% humidity is less than or equal to 57g / m 2 .

[0050] In some embodiments, please refer to Figure 4The display panel 10 further includes a thin film transistor array layer (not shown in the figure) arranged on the side of the first substrate 11 close to the second substrate 12, an insulating layer 51 covering the thin film transistor array layer, a first alignment layer 52 arranged on the side of the insulating layer 51 away from the first substrate 11, and a spacer column 42 arranged on the side of the first alignment layer 52 close to the second substrate 12, and the spacer column 42 is used to support the first substrate 11 and the second substrate 12 to maintain the box thickness of the liquid crystal 41; the display panel 10 further includes a color filter layer 53 arranged on the side of the second substrate 12 close to the first substrate 11, a common electrode layer 54 arranged on the side of the color filter layer 53 away from the second substrate 12, and a second alignment layer 55 arranged on the side of the common electrode layer 54 away from the color filter layer 53.

[0051] As mentioned above, the present application can reduce the curing rate of the epoxy resin polymer in the frame glue 20, thereby reducing the elastic modulus of the frame glue 20 and increasing the flexibility of the frame glue 20, thereby effectively reducing the probability of microcracks appearing at the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12, and reducing the probability of the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12 invading the display panel 10, thereby improving the water-blocking performance of the display panel 10, reducing the probability of adverse phenomena occurring in the display panel 10 due to water vapor intrusion, and improving the stability of the display panel 10.

[0052] In addition, an embodiment of the present application further provides a method for manufacturing a display panel, and the display panel can be Figure 1 The manufacturing method of the display panel 10 shown in the figure comprises the following steps:

[0053] Forming a sealant intermediate on the first substrate 11;

[0054] A liquid crystal 41 is disposed on the first substrate 11, wherein the liquid crystal 41 is located in the area enclosed by the frame glue intermediate body;

[0055] forming a second substrate 12 on the first substrate 11;

[0056] The sealant intermediate connected between the first substrate 11 and the second substrate 12 is cured, wherein the sealant 20 formed after the sealant intermediate is cured includes epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%.

[0057] The present application reduces the curing rate of the epoxy resin polymer in the frame glue 20, thereby reducing the elastic modulus of the frame glue 20 and increasing the flexibility of the frame glue 20, thereby effectively reducing the probability of microcracks appearing at the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12, reducing the probability of the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12 invading the display panel 10, improving the water-blocking performance of the display panel 10, reducing the probability of adverse phenomena occurring in the display panel 10 due to water vapor intrusion, and improving the stability of the display panel 10.

[0058] Please continue to refer to Figure 1 , Figure 4 as well as Figure 5 The manufacturing method of the display panel 10 comprises the following steps:

[0059] S10 , forming a sealant intermediate on the first substrate 11 .

[0060] S20 , disposing a liquid crystal 41 on the first substrate 11 , wherein the liquid crystal 41 is located in a region enclosed by the frame glue intermediate.

[0061] S30 , disposing a second substrate 12 on the first substrate 11 .

[0062] S40, curing the sealant intermediate connected between the first substrate 11 and the second substrate 12, wherein the sealant 20 formed after the sealant intermediate is cured comprises epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%.

[0063] Specifically, in step S10 , the first substrate 11 is provided; in some embodiments, a thin film transistor array layer, an insulating layer 51 , a first alignment layer 52 and spacer columns 42 are disposed on the first substrate 11 .

[0064] A sealant intermediate is formed on the peripheral side of the first substrate 11 on which the first alignment layer 52 is provided, and the sealant intermediate forms an enclosed area on the first substrate 11 .

[0065] In some embodiments, the frame glue intermediate includes acrylic small molecules, epoxy resin, photoinitiator and thermal initiator, wherein the mass fraction of the acrylic small molecules in the frame glue intermediate is 10% to 50%, the mass fraction of the epoxy resin in the frame glue intermediate is 10% to 50%, the mass fraction of the photoinitiator in the frame glue intermediate is 1% to 5%, and the mass fraction of the thermal initiator in the frame glue intermediate is 5% to 15%.

[0066] In some embodiments, the epoxy resin is one or a combination of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol H epoxy resin, novolac epoxy resin, multifunctional glycidyl ether epoxy resin, multifunctional glycidyl amine epoxy resin and halogenated epoxy resin.

[0067] In some embodiments, the photoinitiator includes at least one of the following compounds:

[0068]

[0069] In some embodiments, the thermal initiator includes at least one of the following compounds:

[0070]

[0071] In step S20 , a liquid crystal 41 is formed on the first substrate 11 , and the liquid crystal 41 is located in a region enclosed by the sealant intermediate body.

[0072] In step S30 , a second substrate 12 is provided. In some embodiments, a color filter layer 53 , a common electrode layer 54 and a second alignment layer 55 are disposed on the second substrate 12 .

[0073] The second substrate 12 is formed on one side of the first substrate 11 where the sealant intermediate is provided, and the second substrate 12 is connected to the first substrate 11 through the sealant intermediate, so that the liquid crystal 41 is located in the space enclosed by the first substrate 11, the second substrate 12 and the sealant intermediate.

[0074] In other embodiments, a color filter layer, a common electrode layer and a second alignment layer may be disposed on the first substrate 11 , and a thin film transistor array layer, an insulating layer, a first alignment layer and spacers may be disposed on the second substrate 12 .

[0075] Furthermore, in step S40 , the sealant intermediate connected between the first substrate 11 and the second substrate 12 is cured so that the sealant intermediate is cured to form the sealant 20 , and the sealant 20 is connected between the first substrate 11 and the second substrate 12 .

[0076] In some embodiments, the process of curing the sealant intermediate includes performing a light curing treatment and a heat curing treatment on the sealant intermediate.

[0077] The sealant intermediate is subjected to a light curing treatment, and at least a portion of the acrylic small molecules are polymerized to form acrylic macromolecules, so that the sealant intermediate is basically shaped and has a certain adhesion.

[0078] The sealant intermediate is subjected to heat curing treatment, part of the epoxy resin is polymerized, and part of the unreacted acrylic small molecules are also polymerized to form acrylic polymers, so that the sealant intermediate reacts to form the sealant 20, and the sealant 20 has stronger adhesion, and the first substrate 11 and the second substrate 12 are combined together.

[0079] In some embodiments, the SUV integrated light amount of the photocuring treatment is less than or equal to 3000mj, the temperature of the thermal curing treatment is less than or equal to 120°C, and the duration of the thermal curing treatment is less than 50min. Usually, during the thermal curing process of the frame glue, the temperature will be greater than 120°C and the duration will be greater than or equal to 50 minutes to allow the epoxy resin in the frame glue to fully polymerize. However, the embodiments of the present application require an epoxy resin polymer with a lower curing rate. Therefore, the temperature and duration of the thermal curing treatment in the embodiments of the present application are reduced.

[0080] In some embodiments, in the step of curing the frame glue intermediate, the curing rate of the epoxy resin polymer is greater than or equal to 40% and less than or equal to 50%, for example, it can be 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%; the embodiments of the present application not only improve the flexibility of the frame glue 20, but also need to maintain the mechanical strength of the frame glue 20. Therefore, the curing rate of the epoxy resin polymer also needs to be greater than or equal to 40% to avoid the frame glue 20 being unable to stably connect between the first substrate 11 and the second substrate 12 due to insufficient mechanical strength.

[0081] In some embodiments, the curing rate of the epoxy resin polymer is less than the curing rate of the acrylic. Since the curing rate of the epoxy resin has been reduced in the embodiments of the present application, in order to ensure the mechanical strength and stability of the frame glue 20, the curing rate of the acrylic will at least be maintained from decreasing in the embodiments of the present application; wherein, the curing rate of the acrylic is greater than or equal to 85% and less than or equal to 92%, for example, it can be 85%, 86%, 87%, 88%, 89%, 90%, 91% or 92%.

[0082] It should be noted that the raw material components of the frame glue 20 include epoxy resin, acrylic small molecules, photoinitiator and thermal initiator. The embodiment of the present application improves the flexibility of the frame glue 20 by reducing the curing rate of the epoxy resin polymer, but does not improve the flexibility of the frame glue 20 by reducing the curing rate of the acrylic. It is believed that the curing process of the frame glue 20 generally includes two stages of photocuring and thermal curing, wherein the acrylic small molecules undergo polymerization reaction mainly in the photocuring stage. The present application has been verified to find that if the curing rate of the acrylic small molecules is reduced, the photoinitiator will be precipitated, which will further contaminate the liquid crystal 41. Therefore, in the embodiment of the present application, by making the acrylic have a larger curing rate and reducing the curing rate of the epoxy resin, the precipitation of the photoinitiator can be effectively reduced, and the probability of the liquid crystal 41 being contaminated can be reduced. On this basis, the flexibility of the frame glue 20 can be increased, and the probability of microcracks generated at the interface between the frame glue 20 and the first substrate 11 and the second substrate 12 can be reduced, and the probability of water vapor invading the display panel 10 can be reduced.

[0083] In some embodiments, the curing rate provided in the embodiments of the present application can be determined based on the infrared spectra of the cured sealant and the raw glue; wherein, determining the curing rate of the sealant based on the infrared spectra of the cured sealant and the raw glue can specifically include: integrating the characteristic functional group peaks in the infrared spectra of the cured sealant sample and the raw glue, respectively, and then calculating, and the calculation formula is as follows:

[0084]

[0085] Among them, X represents the curing rate of the sealant, S1 represents the peak area of ​​the target characteristic functional group of the sealant sample, S2 represents the peak area of ​​the reference functional group of the sealant sample, S3 represents the peak area of ​​the target characteristic functional group of the raw rubber, and S4 represents the peak area of ​​the reference functional group of the raw rubber. The reference peak functional group is a benzene ring, and the target peak functional group can be an epoxy group or acryl (acrylic).

[0086] In addition, the embodiments of the present application provide comparative examples 1, 2 and 3, and embodiments 1 to 6 to verify the performance of the sealant 20 .

[0087] In comparative example 1, the SUV integrated light amount during the photocuring treatment is 3000 mj, the temperature during the heat curing treatment is 120° C., the duration of the heat curing treatment is 50 min, and the performance of the frame glue in comparative example 1 is tested.

[0088] In comparative example 2, the SUV integrated light amount during the photocuring treatment is 3000 mj, the temperature during the thermal curing treatment is 120° C., the duration of the thermal curing treatment is 50 min, and the performance of the frame glue in comparative example 2 is tested.

[0089] In comparative example 3, the SUV integrated light amount during the photocuring treatment is 1500 mj, the temperature during the thermal curing treatment is 120° C., and the duration of the thermal curing treatment is 50 min. The performance of the frame glue in comparative example 3 is tested.

[0090] In Example 1, the SUV integrated light amount during the photocuring treatment is 3000 mj, the temperature during the thermal curing treatment is 120° C., the duration of the thermal curing treatment is 30 min, and the performance of the sealant in Example 1 is tested.

[0091] In Example 2, the SUV integrated light amount during the photocuring treatment is 3000 mj, the temperature during the thermal curing treatment is 120° C., the duration of the thermal curing treatment is 30 min, and the performance of the sealant in Example 2 is tested.

[0092] In Example 3, the SUV integrated light amount during the photocuring treatment is 3000 mj, the temperature during the thermal curing treatment is 120° C., the duration of the thermal curing treatment is 30 min, and the performance of the sealant in Example 3 is tested.

[0093] In Example 4, the SUV integrated light amount during the photocuring treatment is 1500 mj, the temperature during the thermal curing treatment is 120° C., the duration of the thermal curing treatment is 30 min, and the performance of the sealant in Example 4 is tested.

[0094] In Example 5, the SUV integrated light amount during the photocuring treatment is 1500 mj, the temperature during the thermal curing treatment is 120° C., the duration of the thermal curing treatment is 30 min, and the performance of the sealant in Example 5 is tested.

[0095] In Example 6, the SUV integrated light amount during the photocuring treatment is 1500 mj, the temperature during the thermal curing treatment is 120° C., the duration of the thermal curing treatment is 30 min, and the performance of the sealant in Example 6 is tested.

[0096] Through the testing of Comparative Examples 1, 2 and 3 and Examples 1 to 6, the data shown in the following Table 1 were obtained.

[0097] Table 1 Test results

[0098]

[0099]

[0100] The elasticity of the sealants in the comparative examples and embodiments can be tested by DMA (dynamic mechanical analysis).

[0101] Adhesion test method: Use plain glass to cross, apply a fixed size of frame glue at the cross position, and use the ejector pin method to test the tensile force of the frame glue under different conditions.

[0102] Moisture permeability test method: prepare a sealant film with a thickness of less than 300um, fix the sealant film in a moisture permeability cup, put 10g CaCl2 in the moisture permeability cup, and place it at high temperature and high humidity (85℃ / 85%RH). Weigh it every 24 hours, fit the weight data such as T0 / T24... / T168 to form a linear trend, and calculate the moisture permeability. Moisture permeability = 24*K (fitting slope) * D (actual film thickness) / 300, unit is g / m 2 , where K refers to the slope of the linear trend of the mass change of CaCl2 collected at different times, and D refers to the actual film thickness of the sealant film prepared for testing moisture permeability.

[0103] It can be seen from Table 1 above that in the embodiment of the present application, the curing rate of the epoxy resin polymer can be effectively reduced by the treatment time during the thermal curing treatment process, and the water vapor test under three conditions can be passed, indicating that the frame glue 20 provided in the embodiment of the present application can effectively improve the water-blocking performance of the display panel 10.

[0104] In summary, the present application reduces the curing rate of the epoxy resin polymer in the frame glue 20, thereby reducing the elastic modulus of the frame glue 20 and increasing the flexibility of the frame glue 20, thereby effectively reducing the probability of microcracks appearing at the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12, and reducing the probability of the connection interface between the frame glue 20 and the first substrate 11 and the second substrate 12 invading the display panel 10, thereby improving the water-blocking performance of the display panel 10, reducing the probability of adverse phenomena occurring in the display panel 10 due to water vapor intrusion, and improving the stability of the display panel 10.

[0105] In addition, an embodiment of the present application further provides a display device, which includes the display panel, or a display panel manufactured using the manufacturing method of the display panel.

[0106] In some embodiments, the display device further includes a backlight module, and the display panel is disposed on a light emitting side of the backlight module.

[0107] It can be understood that, since the display device provided in the embodiment of the present application contains the same display panel as in the above embodiment, the display device has the same beneficial effects as the display panel, which will not be described in detail herein.

[0108] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0109] The above is a detailed introduction to a display panel and a manufacturing method thereof provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solutions and core ideas of the present application. Ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents; and these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A display panel, characterized in that: include: a first substrate; a second substrate, arranged opposite to the first substrate; Frame glue, connected between the first substrate and the second substrate; as well as Liquid crystal is arranged in a space enclosed by the first substrate, the second substrate and the frame glue; The sealant includes epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%.

2. The display panel according to claim 1, characterized in that: The curing rate of the epoxy resin polymer is greater than or equal to 40%.

3. The display panel according to claim 1, characterized in that: The curing rate of the epoxy resin polymer is lower than the curing rate of the acrylic.

4. The display panel according to claim 1, characterized in that: The curing rate of the acrylic is greater than or equal to 85% and less than or equal to 92%.

5. The display panel according to any one of claims 1 to 4, characterized in that: The elastic modulus of the sealant is greater than or equal to 3.1 GPa and less than or equal to 3.4 GPa.

6. The display panel according to any one of claims 1 to 4, characterized in that: The moisture permeability of the sealant is less than or equal to 57g / m 2 .

7. A method for manufacturing a display panel, characterized in that: The following steps are involved: forming a sealant intermediate on the first substrate; Disposing liquid crystal on the first substrate, wherein the liquid crystal is located in the area enclosed by the frame glue intermediate; Disposing a second substrate on the first substrate; The sealant intermediate connected between the first substrate and the second substrate is cured, wherein the sealant formed after the sealant intermediate is cured includes epoxy resin polymer and acrylic, and the curing rate of the epoxy resin polymer is less than or equal to 50%.

8. The method for manufacturing a display panel according to claim 7, characterized in that: The frame glue intermediate includes acrylic small molecules, epoxy resin, photoinitiator and thermal initiator; The curing process of the sealant intermediate connected between the first substrate and the second substrate includes: Performing a light-curing treatment on the sealant intermediate to polymerize at least a portion of the acrylic small molecules; The sealant intermediate is subjected to a heat curing treatment, and a portion of the epoxy resin is polymerized.

9. The method for manufacturing a display panel according to claim 8, characterized in that: The temperature of the thermal curing treatment is less than or equal to 120° C., and the duration of the thermal curing treatment is less than 50 minutes.

10. The method for manufacturing a display panel according to claim 7, characterized in that: In the step of curing the sealant intermediate connected between the first substrate and the second substrate, the curing rate of the epoxy resin polymer is greater than or equal to 40%, and the curing rate of the acrylic is greater than or equal to 85% and less than or equal to 92%.