Design and preparation method of special nickel-based high-temperature alloy for additive material based on data driving
Using a data-driven approach to design additive-specific nickel-based high-temperature alloys, optimizing their composition and process has solved the problem of forming defects in additive manufacturing, improved the structural stability and mechanical properties of high-temperature alloys, and is suitable for the manufacturing of high-temperature parts.
Patent Information
- Application Number
- CN202410539588.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2024-10-11
AI Technical Summary
At this stage, additive manufacturing of nickel-based superalloys has forming defects, such as cracks and holes, resulting in insufficient high-temperature performance and inability to meet actual application needs.
A data-driven approach is used to design additive-specific nickel-based superalloys. By setting the component value range, calculating thermodynamic parameters, training machine learning models, screening alloy components, and combining selective laser melting technology to prepare nickel-based superalloys, the components and Process parameters to reduce defects.
A nearly crack-free, defect-free nickel-based superalloy finished product with a γ′ phase volume fraction of 45% has been achieved, which meets the design requirements, improves structural stability and mechanical properties, and is suitable for additive manufacturing of high-temperature parts.
Smart Images

Figure CN118761304A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of additive manufacturing of nickel-based high-temperature alloys, and specifically refers to a data-driven design and preparation method of a special nickel-based high-temperature alloy for additive manufacturing. Background Art
[0002] Additively manufactured nickel-based superalloy parts have excellent surface accuracy and high forming density, and their mechanical properties such as tensile strength and hardness reach or even exceed the casting standards. They have broad application prospects in the fields of aerospace and energy power. However, at present, the superalloys used in additive manufacturing are mostly alloy grades designed based on traditional forming processes such as casting, forging, and welding, and the alloy composition does not match the characteristics of the additive manufacturing process. Solid solution-strengthened nickel-based superalloys have good formability, such as IN625 and Hastelloy X, but their high-temperature performance is insufficient; γ′ precipitation-strengthened nickel-based superalloys, such as IN738 and CM247LC, have excellent high-temperature performance, but the presence of γ′ phase-forming elements such as Al, Ti, and Ta causes this type of alloy to be prone to a large number of cracks, holes and other defects during additive manufacturing, making it impossible to form and apply. Therefore, it is urgent to develop a design and preparation method for nickel-based superalloys suitable for additive manufacturing, which can improve the defects of nickel-based superalloy additive manufacturing and meet the needs of practical applications. Summary of the invention
[0003] The purpose of the present invention is to provide a data-driven design and preparation method for a nickel-based high-temperature alloy specifically for additive manufacturing, which can improve the defects of nickel-based high-temperature alloy additive manufacturing and meet the needs of practical applications.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] In a first aspect, the present invention provides a data-driven design method for additive-specific nickel-based high-temperature alloys, comprising the following steps:
[0006] S1. Generate a component space by setting a value range of the nickel-based high-temperature alloy composition;
[0007] S2. Establish a data set by calculating the thermodynamic parameters A of the component space, wherein the thermodynamic parameters A include: γ′ phase solid solution temperature T γ′ , the difference between the solidus temperature and the γ′ phase solution temperature T S -T γ′ , γ′ phase volume fraction V under high temperature conditions γ′ and TCP phase volume fraction V TCP ; The high temperature condition is any temperature between 650-1100°C;
[0008] S3. training a machine learning model through the data set to obtain a relationship model between the nickel-based high-temperature alloy composition and the thermodynamic parameter A, and screening candidate alloy compositions by taking the threshold of the thermodynamic parameter A as a constraint;
[0009] S4. By calculating the thermodynamic parameter B of the candidate alloy component, the crack resistance factor of the candidate alloy component is obtained, and the target alloy component is screened by taking the threshold value of the crack resistance factor as a constraint, wherein the thermodynamic parameter B includes: liquid phase molar fraction N L , liquid phase molar volume N VL , system molar volume N V and solid phase solidification path F S The anti-cracking factor includes: solidification temperature range T SL , solidification rate SCI in critical temperature range, total strain of solidification shrinkage ε, maximum strain rate ε max and the average rate of change of liquid volume fraction with temperature V rate .
[0010] Optionally, in step S1, a component space is generated by setting a value range of the nickel-based high-temperature alloy composition, including:
[0011] S1-1. According to the range of nickel-based high-temperature alloy components, elements including Ni and Co, Mo, Cr, W, V, Al, Ti, Ta, Nb, C and B are pre-selected as nickel-based high-temperature alloy components. In terms of mass percentage, the preset range of each element is Co: 0-25%, Mo: 0-5%, Cr: 0-20%, W: 0-8%, V: 0-2%, Al: 0-6%, Ti: 0-6%, Ta: 0-8%, Nb: 0-8%, C: 0-0.5%, B: 0-0.1%, and the balance is Ni;
[0012] S1-2. Generate the component space by performing fixed-step sampling or random sampling on a preset range of each element.
[0013] Optionally, in step S3, a machine learning model is trained by the data set to obtain a relationship model between the nickel-based high-temperature alloy composition and the thermodynamic parameter A, and a candidate alloy composition is screened by taking a threshold value of the thermodynamic parameter A as a constraint, including:
[0014] S3-1. By taking the alloy composition as input and the thermodynamic parameter A as output, a machine learning model is established, and the machine learning model is trained using the data set based on a regression method to obtain the R of the thermodynamic parameter A. 2 All reach above 0.9, the training is finished, and the relationship model between the composition of the nickel-based high-temperature alloy and the thermodynamic parameter A is obtained; the R 2 The calculation formula is:
[0015]
[0016] Among them, Y i represents the true value of the i-th sample, represents the model prediction value of the i-th sample, is the average of the true values, and n is the number of data samples;
[0017] S3-2. By using the threshold value of the thermodynamic parameter A as a constraint, candidate alloy components are screened; the threshold value of the thermodynamic parameter A is: T γ′ >1100℃、T S -T γ′ >50℃、0.40≤V γ′ ≤0.70, V TCP <0.1.
[0018] Optionally, in step S4, the anti-cracking factor of the candidate alloy component is obtained by calculating the thermodynamic parameter B of the candidate alloy component, and the target alloy component is screened by taking the threshold of the anti-cracking factor as a constraint, including:
[0019] S4-1. Calculate the thermodynamic parameters B of the candidate alloy composition by thermodynamic calculation software, and save the thermodynamic parameters B as liquid phase mole fraction N corresponding to temperature T. L File, liquid phase molar volume N VL File, system molar volume N V File and solid phase solidification path F S File, calculate the anti-cracking factor T SL 、SCI、ε、ε max and V rate ,include:
[0020] F4-1.T SL =T L -T S ; T L represents the alloy liquidus temperature, T S represents the alloy solidus temperature;
[0021] F4-2. fs is the solid fraction, and the value range of fs is 0.9-0.99. It indicates the rate of change of temperature with solid phase fraction during alloy solidification;
[0022] F4-3. V i The volume fraction of the liquid phase is i, T i is the temperature corresponding to the liquid volume fraction i, V iThe value range is 20% to 3%;
[0023] F4-4. dV system The system is at temperature T i Volume change when the temperature drops by 2℃, V system Corresponding to temperature T i Total system volume;
[0024] F4-5. ε max represents the maximum strain rate of the alloy at the end of solidification, V i The value range is 2%-10%;
[0025] S4-2. The target alloy composition is obtained by screening the threshold value of the anti-crack factor as a constraint, and the threshold value of the anti-crack factor is: T SL <310、SCI<3000、V rate <0.151、ε<0.011、ε max <0.002.
[0026] Optionally, in F4-1, by reading the solid phase solidification path F S file, when fs is positive and minimum, it corresponds to fs L , fs L The corresponding temperature is T L , the last fs in the file corresponds to fs s , fs s The corresponding temperature is T S , calculate T SL =T L -T S .
[0027] Optionally, in F4-2, by reading the solid phase solidification path F S File, extract fs between fs=0.9-0.99 and the corresponding temperature T, calculate SCI n-1 =(T n-1 -T n ) / (fs n 1 / 2 -fs n-1 1 / 2 ), SCI=(SCI1+SCI2……SCI n-1 ) / (n-1).
[0028] Optionally, in F4-3, read the liquid phase mole fraction N L File, liquid phase molar volume N VL File and system molar volume N V File, extract N L 、NVL and N V With the corresponding temperature T, calculate V i =N L *(N VL / N V ), extract to V i The temperatures T closest to 0.2, 0.1, 0.03, and 0.02 are recorded as T1, T2, T3, and T4, respectively, where the magnitude relationship is T1>T2>T3>T4. At this time, V rate =17 / (T1-T3).
[0029] Optionally, in F4-4, read the system molar volume N V All T values and corresponding N values of temperature T1 and below obtained in the file V Value, adjacent N V A component ε is calculated between the values k =ABS(N Vn+1 -N Vn ) / N Vn , calculate all components εk below temperature T1, and then take all components ε between T1 and T3 k The sum of is ε.
[0030] Optionally, in F4-5, according to each component ε k The corresponding temperature T can be further calculated as the component ε at the corresponding temperature rate , ε rate =ABS(ε k -ε k+1 ) / (T n -T n+1 ), after calculating all components ε below T2 rate After that, ε max is all components ε between T2 and T4 rate The maximum value of .
[0031] In a second aspect, the present invention provides a method for preparing a nickel-based high-temperature alloy, which is prepared according to the target alloy composition obtained by the aforementioned data-driven additive-specific nickel-based high-temperature alloy design method, and comprises the following steps:
[0032] P1. Melting the master alloy, weighing the ingredients according to the target alloy composition of the nickel-based high-temperature alloy, and melting the weighed raw materials to prepare the master alloy;
[0033] P2. Gas atomization powdering, wherein the master alloy is gas atomized to prepare an alloy powder;
[0034] P3. The alloy powder is printed layer by layer using the selective laser melting technology to prepare a nickel-based high-temperature alloy.
[0035] In summary, the present invention has at least one of the following beneficial effects:
[0036] The data-driven design method for additive-specific nickel-based high-temperature alloys provided by the present invention uses thermodynamic calculation software to calculate the thermodynamic parameters of high-temperature alloys with multi-element components and large composition space, obtains a massive composition-thermodynamic parameter database, and establishes a high-precision composition-thermodynamic parameter machine learning model. The model is used to constrain thermodynamic parameters (including phase and thermophysical parameters) to achieve spatial optimization design of alloy components with stable organization and excellent mechanical properties. Solidification parameter calculation is carried out in combination with the non-equilibrium solidification characteristics of additive manufacturing. According to the existing application of high-temperature alloy additives, the optimal design is constrained by 5 anti-cracking factors to obtain the composition of nickel-based high-temperature alloys for additives. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 A flow chart of a data-driven design method for additive-specific nickel-based high-temperature alloys provided in one embodiment of the present invention;
[0039] Figure 2 R is the prediction result of the neural network model of the composition and thermodynamic parameters of the nickel-based high-temperature alloy in a specific embodiment of the present invention 2 Numeric value;
[0040] Figure 3 To invent a specific embodiment of a new nickel-based high-temperature alloy additive manufacturing different cross-sectional microstructure morphology diagram;
[0041] Figure 4 This is a γ′ phase microstructure diagram of a novel nickel-based high-temperature alloy according to a specific embodiment of the invention. DETAILED DESCRIPTION
[0042] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0043] The present invention proposes a data-driven design method for additive-specific nickel-based high-temperature alloys. Based on the knowledge in the field of materials science and the characteristics of non-equilibrium solidification, a model of nickel-based high-temperature alloy composition and thermodynamic parameters is established through machine learning to assist in the spatial screening of alloy components with stable organization and high performance. Furthermore, 5 anti-cracking factor constraints are calculated and proposed to screen and obtain the additive-specific nickel-based high-temperature alloy composition. The selective laser melting technology (SLM) additive preparation of the target component alloy is completed, and the detection shows that there are almost no crack defect characteristics, and the volume fraction of the γ′ phase reaches 45%, which meets the design requirements. The invention is conducive to the development of additive-specific high-temperature alloy compositions and accelerates the promotion and application of high-temperature components of additively manufactured high-temperature alloys with stable organization, excellent mechanical properties, and crack-free. The flow chart of the data-driven design method for additive-specific nickel-based high-temperature alloys according to the embodiment of the present invention is as follows: Figure 1 As shown, the details are as follows:
[0044] S1. Generate component space by setting the value range of nickel-based high-temperature alloy composition, including:
[0045] S1-1. According to the range of nickel-based high-temperature alloy components, elements including Ni and Co, Mo, Cr, W, V, Al, Ti, Ta, Nb, C and B are pre-selected as nickel-based high-temperature alloy components. In terms of mass percentage, the preset range of each element is Co: 0-25%, Mo: 0-5%, Cr: 0-20%, W: 0-8%, V: 0-2%, Al: 0-6%, Ti: 0-6%, Ta: 0-8%, Nb: 0-8%, C: 0-0.5%, B: 0-0.1%, and the balance is Ni. Among them, Co, Mo, Cr, W, and V are selected as solid solution strengthening elements to improve the high-temperature strength of the alloy, Al, Ti, Ta, and Nb are selected as the forming elements of γ′ phase (Ni3(Al,Ti)) or γ″ phase (Ni3Nb), and C and B elements are used as grain boundary strengthening elements to improve the high-temperature creep performance of the alloy. In a specific embodiment of the present invention, the value range of each element is shown in Table 1, and all data are in mass percentage wt.%.
[0046] Table 1 Value range of each element in nickel-based high-temperature alloy
[0047]
[0048] S1-2. Generate the component space by performing fixed step sampling or random sampling on the preset range of each element. In a specific embodiment of the present invention, Python is used to randomly sample and generate 60,000 groups of component spaces within the range of Table 1 to obtain a large amount of high-temperature alloy composition and thermodynamic parameter data.
[0049] S2. Establish a data set by calculating the thermodynamic parameters A of the component space, wherein the thermodynamic parameters A include: γ′ phase solid solution temperature Tγ′ , the difference between the solidus temperature and the γ′ phase solution temperature T S -T γ′ , γ′ phase volume fraction V under high temperature conditions γ′ and TCP phase volume fraction V TCP ;include:
[0050] S2-1. The high temperature condition is set according to the application temperature of the nickel-based high temperature alloy, and the high temperature condition is any temperature between 650-1100° C. In a specific embodiment of the present invention, the high temperature condition is selected to be 900° C.
[0051] S2-2. Calculate the thermodynamic parameter A of the component space under the high temperature condition by thermodynamic calculation software, and establish a data set of alloy composition-thermodynamic parameter. In a specific embodiment of the present invention, the TCNI9 database in the Thermo-Calc thermodynamic software is used to calculate the γ′ phase solution temperature T of each group of alloy components in the above-mentioned component space. γ′ , Heat treatment temperature window (T S -T γ′ ), γ′ phase and TCP phase fraction V at 900℃ γ′ and V TCP These four thermodynamic parameters construct a data set of alloy composition-thermodynamic parameters. In order to simplify the calculation of thermodynamic parameters and improve the calculation accuracy, the main phase and the phase with high probability are input into the Thermo-Calc thermodynamic software for calculation through screening, including Liquid (liquid phase), fcc_L12 (γ and γ′ phases), C14_LAVES (Laves phase), M 23 C6(M 23 C6 phase), HCP_A3 (HCP phase), NI3TA_D0A (Ni3Ta phase), NI3TI_D024 (Ni3Ti phase), MC_ETA (MC phase), M3B2_TETR (M3B2 phase), MU_PHASE (μ phase) and P_PHASE (P phase). It can be obtained that the volume fraction of TCP phase V TCP =C14_LAVES (Laves phase) volume fraction + MU_PHASE (μ phase) volume fraction + P_PHASE (P phase) volume fraction.
[0052] S3. Training a machine learning model with the data set to obtain a relationship model between the nickel-based high-temperature alloy composition and the thermodynamic parameter A, and screening candidate alloy compositions using the threshold of the thermodynamic parameter A as a constraint, including:
[0053] S3-1. By taking the alloy composition as input and the thermodynamic parameter A as output, a machine learning model is established, and the machine learning model is trained using the data set based on a regression method to obtain the R of the thermodynamic parameter A. 2 All reach above 0.9, the training is finished, and the relationship model between the composition of the nickel-based high-temperature alloy and the thermodynamic parameter A is obtained; the R 2 The calculation formula is:
[0054]
[0055] Among them, Y i represents the true value of the i-th sample, represents the model prediction value of the i-th sample, is the average value of the true value, and n is the number of data samples. In a specific embodiment of the present invention, the machine learning model adopts a neural network model, and adopts a mathematical method Z-Score method to eliminate the influence of scale differences between data. This method can scale the alloy composition and the four thermodynamic parameters A in the component space to standard data with an average value of 0 and a standard deviation of 1. The specific formula is as follows:
[0056]
[0057] Z is the standardized value; x is the original data; is the average value of the original data; σ is the standard deviation of the corresponding original data, and 60,000 sets of standard data are obtained. The selected training set is 70% randomly selected from the 60,000 sets of standard data, and the remaining 30% is used as the validation set. 2 In the range of [0,1], it is an evaluation index. The R of a training target 2 The closer the value is to 1, the higher the prediction accuracy of the target in the model. In a specific embodiment of the present invention, a single hidden layer and 30 neurons are selected as the final neural network model. After the model training is completed, the R values of the four thermodynamic parameters are 2 The value fluctuations are small and are all above 0.9. Figure 2 shown.
[0058] S3-2. By using the threshold value of the thermodynamic parameter A as a constraint, candidate alloy components are screened; the threshold value of the thermodynamic parameter A is: T γ′ >1100℃、T S -T γ′ >50℃、0.40≤V γ′ ≤0.70, V TCP <0.1. The mechanical properties of high-temperature alloys are closely related to their internal microstructure. In order to ensure the structural stability of high-temperature alloys, the γ′ phase solid solution temperature T γ′It must be higher than the service temperature. The service temperature of precipitation-strengthened high-temperature alloys is generally between 900°C and 1000°C. If the γ′ phase solution temperature is close to the above range, the γ′ phase will be mostly or even completely dissolved into the matrix, and the high-temperature strength of the material will be completely lost. Therefore, the γ′ phase solution temperature parameter is set to be greater than 1100°C, that is, T γ′ >1100°C, in one embodiment of the present invention, T γ′ >1120℃. It is difficult to obtain a γ′ phase with uniform structure and particle size that meets the requirements for γ′ strengthened high temperature alloys under the conditions of rapid heating and cooling in additive manufacturing. After additive manufacturing, corresponding heat treatment processes are required to achieve γ′ phase structure control and obtain excellent performance. Therefore, a wide heat treatment window is conducive to post-additive heat treatment. The heat treatment temperature window is designed to be greater than 50℃, that is, T S -T γ′ >50℃. High γ′ phase content high temperature alloys have better mechanical properties, which often means that they contain more Al, Ti, and Ta elements. The presence of these elements increases the cracking sensitivity of the additive process. To ensure the feasibility of additive manufacturing, according to the existing research on the content of γ′ phase in additive manufacturing, its volume fraction space is determined, that is, 0.40≤V γ′ ≤0.70, and in one embodiment of the present invention, 0.45≤V γ′ ≤0.65. A large amount of refractory elements are added to high-temperature alloys, but too much refractory elements can easily promote the precipitation of harmful TCP phases. The brittle TCP phase will lead to a decrease in its high-temperature performance and reduce the thermal stability of the high-temperature alloy. Therefore, its precipitation should be controlled as much as possible, that is, V TCP <0.1, in a specific implementation of the present invention, V TCP <0.05.
[0059] In order to obtain more data, the Monte Carlo method was used to randomly generate 10 7 The random components were brought into the neural network model and conditionally constrained by thermodynamic parameters, and finally 10159 groups of candidate alloys were obtained, which met the thermodynamic parameter constraints.
[0060] S4. Obtaining the anti-cracking factor of the candidate alloy component by calculating the thermodynamic parameter B of the candidate alloy component, and screening the target alloy component by taking the threshold of the anti-cracking factor as a constraint, including:
[0061] S4-1. Calculate the thermodynamic parameters B of the candidate alloy composition by thermodynamic calculation software, wherein the thermodynamic parameters B include: solid phase solidification path F S , liquid phase mole fraction N L , liquid phase molar volume N VL and the system molar volume N V, export the EXP files of the four thermodynamic parameters B of each alloy, the file name format is NiAlloy number_Fs, NiAlloy number_NVL, NiAlloy number_NV, NiAlloy number_NL, where the number is the number of alloys, from 1 to 10159, indicating that there are 10159 alloys. In the four EXP files, the data is divided into two columns, one for temperature T and one for the corresponding calculated value, and the two columns of data correspond one to one. Calculate the anti-cracking factor, the anti-cracking factor includes: solidification temperature range T SL , solidification rate SCI in critical temperature range, total strain of solidification shrinkage ε, maximum strain rate ε max and the average rate of change of liquid volume fraction with temperature V rate ,include:
[0062] F4-1.T SL =T L -T S ;
[0063] T L represents the alloy liquidus temperature, T S Indicates the alloy solidus temperature, and the difference between the two indicates the alloy solidification range. A smaller solidification range is conducive to liquid phase shrinkage between solidifying dendrites. Specifically, the NiAlloy digital_Fs file includes two columns of data, the left column is fs (0 < fs < 1), fs is the solid phase fraction, and the right column is the temperature T. fs corresponds to T one by one. By reading the solid phase solidification path F S file, when fs is positive and minimum, it corresponds to fs L , fs L The corresponding temperature is T L , at the end of the file, you need to extract the last fs value, recorded as fs S , the corresponding temperature is T S , fs S Generally close to 0.99, solidification interval T SL =T L -T S .
[0064] F4-2.
[0065] The SCI value can reflect the rate of change of temperature with solid phase fraction during alloy solidification, and its magnitude is the absolute value of the change rate. It indicates the rate of change of temperature with solid fraction during alloy solidification. fs indicates the solid fraction. In the critical temperature range (fs = 0.9-0.99), the larger the SCI value, the greater the temperature gradient required to decrease for each unit increase in the alloy solid fraction, which indicates that the alloy solidifies more slowly. The growth rate between adjacent grains slows down, delaying the bonding force between grains required to resist cracks; at the same time, the intergranular channels become longer, hindering the liquid shrinkage required to resist cracks. Specifically, by reading the solid phase solidification path F S In the NiAlloy digital_Fs file, find all the data of fs between 0.9 and 0.99 and the corresponding T and extract them for calculation, SCI1 = (T1-T2) / (fs2 1 / 2 -fs1 1 / 2 ), SCI2=(T2-T3) / (fs3 1 / 2 -fs2 1 / 2 ), ... SCI n-1 =(T n-1 -T n ) / (fs n 1 / 2 -fs n-1 1 / 2 ),SCI=(SCI1+SCI2+……SCI n-1 ) / (n-1), that is, the average value of all SCIs is obtained in the end.
[0066] F4-3.
[0067] V i The volume fraction of the liquid phase is i, T i is the temperature corresponding to the liquid volume fraction i, V rate represents the liquid volume fraction (V i =20%~3%) with the average rate of change of temperature. Specifically, we need to extract the data of NiAlloy Digital_NVL, NiAlloy Digital_NV, and NiAlloy Digital_NL files and calculate them with each other. The left column is the temperature T, and the right column is the corresponding N VL 、N V 、N L The T values in the left column of the three files are the same. These three files need to extract all the temperatures T, N L 、N VL 、N V There are four columns of data in total, and the four columns of data correspond to each other. L 、N VL 、N V The calculation is performed between each of the three columns of data, and the formula is V i =N L*(N VL / N V ), the new data column generated will also be related to temperature T, N L 、N VL 、N V These four columns correspond one to one, and the value of the new data column will gradually change from 1 to 0. At this time, you need to find the V in the new data column. i The temperatures closest to 0.2, 0.1, 0.03, and 0.02 are recorded as T1, T2, T3, and T4, respectively, where the magnitude relationship is T1>T2>T3>T4. At this time, V rate =17 / (T1-T3).
[0068] F4-4.
[0069] V system is the total volume of the system (corresponding to temperature T i ), dV system The system is at temperature T i The volume change when the temperature is reduced by 2℃. Specifically, the calculation of ε requires the extraction of data in the NiAlloy digital_NV file. At this time, it is necessary to extract all T values and the corresponding N values of the temperature T1 and below obtained in F4-3. V Value, adjacent N V A component ε can be calculated between the values k =ABS(NV n+1 -NV n ) / NV n , all components ε below temperature T1 k All need to be calculated, and then take all components ε between T1 and T3 k The sum of is ε.
[0070] F4-5.
[0071] ε max Indicates the end of solidification (V i =2%-10%) of the maximum strain rate of the alloy. Specifically, all components ε below temperature T1 have been calculated in F4-4. k , and according to each component ε k The corresponding temperature T can be further calculated as the component ε at the corresponding temperature rate , ε rate =ABS(ε k -ε k+1 ) / (T n -T n+1 ), after calculating all components ε below T2 rate After that, ε max is all components ε between T2 and T4rate The maximum value of .
[0072] S4-2. The target alloy composition is obtained by screening the threshold of the anti-crack factor as a constraint. In a specific embodiment of the present invention, according to the current status of additive manufacturing of nickel-based high-temperature alloys reported, the corresponding five anti-crack factors are calculated, and combined with the additive manufacturing formability analysis, as shown in Table 2, combined with data analysis, the anti-crack factor thresholds are set as follows: T SL <310、SCI<3000、V rate <0.151、ε<0.011、ε max <0.002.
[0073] Table 2 Additive forming of nickel-based superalloys and their calculated crack resistance factors
[0074] Brand TSI SCI <![CDATA[V rate ]]> ε <![CDATA[ε max ]]> Forming ability ABD-850AM 299 3566 0.107 0.0094 0.0022 good ABD-900AM 304 3251 0.111 0.00874 0.00165 good WSU 150 214 2928 0.177 0.00832 0.00065 good Alloy2 241 2865 0.139 0.00838 0.00129 good ExpAM 250 2986 0.131 0.01399 0.0081 good IN625 278 3062 0.0982 0.01605 0.0064 good IN718 227 1917 0.170 0.00929 <![CDATA[9.2E -05 ]]> good InconelX-750 131 2168 0.309 0.00728 <![CDATA[1.7E -05 ]]> good IN738LC 295 5172 0.116 0.00508 0.0017 Difference IN939 363 7797 0.112 0.00639 <![CDATA[5.5E -05 ]]> Difference Astroloy 332 6355 0.111 0.016 0.0084 Difference CM247LC 414 10822 0.0530 0.0576 1.45 Difference CMSX-4 338 10294 0.126 0.00802 <![CDATA[7.0E -05 ]]> Difference Haynes282 399 11437 0.102 0.00912 0.00058 Difference IN100 398 11143 0.0976 0.0144 0.00508 Difference IN713C 435 15645 0.157 0.00618 <![CDATA[1.6E -05 ]]> Difference
[0075] Focusing on five anti-cracking factors, a layer-by-layer screening method was used to obtain 47 nickel-based high-temperature alloys with different compositions. One of the components was selected for additive powder preparation based on cost selection and element requirements, and additive manufacturing verification tests were carried out.
[0076] The specific alloy composition is (wt.%): Al: 5.10%, Ti: 0.52%, Ta: 5.50%, Nb: 1.60%, W: 2.50%, Mo: 1.10%, Co: 20.40%, Cr: 10.7%, C: 0.09%, V: 0.41%, B: 0.0082%, and the balance is Ni.
[0077] The specific preparation steps for additive manufacturing include:
[0078] P1. Melting the master alloy, weighing the ingredients according to the target alloy composition of the nickel-based high-temperature alloy, and melting the weighed raw materials to prepare the master alloy;
[0079] P2. Gas atomization powdering, the master alloy is gas atomized to prepare alloy powder; the external morphology of the prepared alloy powder is nearly spherical, alloy powder D 50 =32.32μm, powder flowability: 16.21s / 50g, bulk density 120.23g / 25ml, oxygen content 160ppm.
[0080] P3. The alloy powder was printed layer by layer by selective laser melting technology to prepare a nickel-based high-temperature alloy. The process parameters of selective laser melting were as follows: laser power 260 W, scanning speed 1000 mm / s, scanning spacing 75 μm, and powder thickness 40 μm.
[0081] An optical microscope is used to observe the cross-sectional defects of the additive samples parallel to and perpendicular to the additive direction, such as Figure 3 As shown in Figure 1, no matter the cross section parallel to the material addition direction or the cross section perpendicular to the material addition direction, there is no obvious crack defect, which meets the design goal. Figure 4 As shown in Table 3, the γ′ phase was observed and statistically analyzed using Image J software. The volume fraction of the γ′ phase of the new high-temperature alloy after heat treatment can reach 45%, and the TCP content is less than 0.01%, which meets the design requirements. The mechanical properties of the nickel-based high-temperature alloy prepared by selective laser melting were characterized, as shown in Table 3.
[0082] Table 3 Mechanical properties of nickel-based high-temperature alloys
[0083]
[0084]
[0085] The present invention proposes a data-driven design method for nickel-based high-temperature alloys specifically for additive manufacturing. By utilizing thermodynamic calculation data, a large amount of composition-thermodynamic performance data is obtained, and a high-precision machine learning model of alloy composition-thermodynamic parameters is constructed. Based on the knowledge in the field of materials science and with physical phases and thermophysical parameters as constraints, the alloy composition with stable organization and excellent mechanical properties is optimized. Further, based on the above-mentioned composition space and combined with the non-equilibrium solidification characteristics of the high-temperature alloy additive process, five anti-cracking factors are calculated, and the constraint threshold is given to optimize the composition of the nickel-based high-temperature alloy specifically for additive manufacturing.
[0086] The above is a detailed introduction to a data-driven additive-specific nickel-based high-temperature alloy design method provided by the present invention. This article uses specific examples to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A data-driven design method for additive-specific nickel-based high-temperature alloys, characterized in that: The steps include: S1. Generate a component space by setting a value range of the nickel-based high-temperature alloy composition; S2. Establish a data set by calculating the thermodynamic parameters A of the component space, wherein the thermodynamic parameters A include: γ′ phase solid solution temperature T γ′ , the difference between the solidus temperature and the γ′ phase solution temperature T S -T γ′ , γ′ phase volume fraction V under high temperature conditions γ′ and TCP phase volume fraction V TCP ; The high temperature condition is any temperature between 650-1100°C; S3. training a machine learning model through the data set to obtain a relationship model between the nickel-based high-temperature alloy composition and the thermodynamic parameter A, and screening candidate alloy compositions by taking the threshold of the thermodynamic parameter A as a constraint; S4. By calculating the thermodynamic parameter B of the candidate alloy component, the crack resistance factor of the candidate alloy component is obtained, and the target alloy component is screened by taking the threshold value of the crack resistance factor as a constraint, wherein the thermodynamic parameter B includes: liquid phase molar fraction N L , liquid phase molar volume N VL , system molar volume N V and solid phase solidification path F S The anti-cracking factor includes: solidification temperature range T SL , solidification rate SCI in critical temperature range, total strain of solidification shrinkage ε, maximum strain rate ε max and the average rate of change of liquid volume fraction with temperature V rate .
2. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 1 is characterized in that: In step S1, a component space is generated by setting a value range of the nickel-based high-temperature alloy composition, including: S1-1. According to the range of nickel-based high-temperature alloy components, elements including Ni and Co, Mo, Cr, W, V, Al, Ti, Ta, Nb, C and B are pre-selected as nickel-based high-temperature alloy components. In terms of mass percentage, the preset range of each element is Co: 0-25%, Mo: 0-5%, Cr: 0-20%, W: 0-8%, V: 0-2%, Al: 0-6%, Ti: 0-6%, Ta: 0-8%, Nb: 0-8%, C: 0-0.5%, B: 0-0.1%, and the balance is Ni; S1-2. Generate the component space by performing fixed-step sampling or random sampling on a preset range of each element.
3. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 1 or 2, characterized in that: In step S3, a machine learning model is trained by the data set to obtain a relationship model between the nickel-based high-temperature alloy composition and the thermodynamic parameter A, and a candidate alloy composition is screened by taking the threshold of the thermodynamic parameter A as a constraint, including: S3-1. By taking the alloy composition as input and the thermodynamic parameter A as output, a machine learning model is established, and the machine learning model is trained using the data set based on a regression method to obtain the R of the thermodynamic parameter A. 2 All reach above 0.9, the training is finished, and the relationship model between the composition of the nickel-based high-temperature alloy and the thermodynamic parameter A is obtained; the R 2 The calculation formula is: Among them, Y i represents the true value of the i-th sample, represents the model prediction value of the i-th sample, is the average of the true values, and n is the number of data samples; S3-2. By using the threshold value of the thermodynamic parameter A as a constraint, candidate alloy components are screened; the threshold value of the thermodynamic parameter A is: T γ′ >1100℃、T S -T γ′ >50℃、0.40≤V γ′ ≤0.70, V TCP <0.
1.
4. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 1 or 2, characterized in that: In step S4, the anti-cracking factor of the candidate alloy component is obtained by calculating the thermodynamic parameter B of the candidate alloy component, and the target alloy component is screened by taking the threshold of the anti-cracking factor as a constraint, including: S4-1. The thermodynamic parameter B of the candidate alloy component is calculated by thermodynamic calculation software, and the thermodynamic parameter B is saved as the liquid phase mole fraction N corresponding to the temperature T. L File, liquid phase molar volume N VL File, system molar volume N V File and solid phase solidification path F S File, calculate the anti-cracking factor T SL 、SCI、ε、ε max and V rate ,include: F4-1.T SL =T L -T S ; T L represents the alloy liquidus temperature, T S represents the alloy solidus temperature; F4-2. fs is the solid fraction, and the value range of fs is 0.9-0.
99. It indicates the rate of change of temperature with solid phase fraction during alloy solidification; F4-3. V i The volume fraction of the liquid phase is i, T i is the temperature corresponding to the liquid volume fraction i, V i The value range is 20% to 3%; F4-4. dV system The system is at temperature T i Volume change when the temperature drops by 2℃, V system Corresponding to temperature T i Total system volume; F4-5. ε max represents the maximum strain rate of the alloy at the end of solidification, V i The value range is 2%-10%; S4-2. The target alloy composition is obtained by screening the threshold value of the anti-crack factor as a constraint, and the threshold value of the anti-crack factor is: T SL <310、SCI<3000、V rate <0.151、ε<0.011、ε max <0.
002.
5. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 4 is characterized in that: In F4-1, by reading the solid phase solidification path F S file, when fs is positive and minimum, it corresponds to fs L , fs L The corresponding temperature is T L , the last fs in the file corresponds to fs s , fs s The corresponding temperature is T S , calculate T SL =T L -T S .
6. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 4, characterized in that: In F4-2, by reading the solid phase solidification path F S File, extract fs between fs=0.9-0.99 and the corresponding temperature T, calculate SCI n-1 =(T n-1 -T n ) / (fs n 1 / 2 -fs n-1 1 / 2 ), SCI=(SCI1+SCI2……SCI n-1 ) / (n-1).
7. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 6, characterized in that: In F4-3, by reading the liquid phase mole fraction N L File, liquid phase molar volume N VL File and system molar volume N V File, extract N L 、N VL and N V With the corresponding temperature T, calculate V i =N L *(N VL / N V ), extract to V i The temperatures T closest to 0.2, 0.1, 0.03, and 0.02 are recorded as T1, T2, T3, and T4, respectively, where the magnitude relationship is T1>T2>T3>T4. At this time, V rate =17 / (T1-T3).
8. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 7, characterized in that: In F4-4, by reading the system molar volume N V All T values and corresponding N values of temperature T1 and below obtained in the file V Value, adjacent N V A component ε is calculated between the values k =ABS(N Vn+1 -N Vn ) / NV n , calculate all components εk below temperature T1, and then take all components ε between T1 and T3 k The sum of is ε.
9. The data-driven design method for additive-specific nickel-based high-temperature alloy according to claim 8, characterized in that: In F4-5, according to each component ε k The corresponding temperature T can be further calculated as the component ε at the corresponding temperature rate , ε rate =ABS(ε k -ε k+1 ) / (T n -T n+1 ), after calculating all components ε below T2 rate After that, ε max is all components ε between T2 and T4 rate The maximum value of .
10. A method for preparing a nickel-based high-temperature alloy, comprising preparing the alloy according to the target alloy composition obtained by the data-driven additive-specific nickel-based high-temperature alloy design method according to claims 1 to 9, characterized in that: The steps include: P1. Melting the master alloy, weighing the ingredients according to the target alloy composition of the nickel-based high-temperature alloy, and melting the weighed raw materials to prepare the master alloy; P2. Gas atomization powdering, wherein the master alloy is gas atomized to prepare an alloy powder; P3. The alloy powder is printed layer by layer using the selective laser melting technology to prepare a nickel-based high-temperature alloy.